一种铝合金材料及其制备方法和应用
By introducing Mg₂Si and Al₂Cu phases into aluminum alloy materials and performing appropriate heat treatment, the problems of insufficient strength and electrical conductivity of aluminum alloy materials are solved, and a high-strength and high-electrical-conductivity aluminum alloy is prepared, which is suitable for new energy vehicle parts.
Patent Information
- Application Number
- CN202311443682.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-09
- Filing Date
- 2023-11-01
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-01
AI Technical Summary
Existing aluminum alloy materials are insufficient in balancing strength and electrical conductivity, and cannot meet the high strength and high electrical conductivity requirements of aluminum alloy rotors for new energy vehicles.
By simultaneously introducing Mg₂Si and Al₂Cu phases into aluminum alloy materials, controlling their content range, and combining them with appropriate heat treatment processes, a strengthening phase combination is formed, thus preparing aluminum alloy materials with both high strength and high electrical conductivity.
It achieves an electrical conductivity ≥48% IACS, yield strength ≥120MPa, tensile strength ≥180MPa, elongation ≥10% for aluminum alloy materials, and a yield strength attenuation rate ≤10% after 100h heat treatment at 180℃. It is suitable for manufacturing vehicle parts such as motor rotors, stators, busbars and inverters.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure BDA0004527160010000021
Abstract
Description
Technical Field
[0001] This invention belongs to the field of aluminum alloy technology, specifically relating to an aluminum alloy material, its preparation method, and its application. Background Technology
[0002] Aluminum alloys, with their high specific strength, low cost, and high recyclability, are gradually replacing copper alloys as the primary material for automotive motor rotors. Currently, common rotor manufacturing methods include centrifugal casting and high-pressure casting, with the former being widely used due to its lower porosity and higher material density. With the development of new energy vehicles, higher requirements are being placed on the strength and electrical conductivity of aluminum alloy rotors.
[0003] To obtain high-strength and high-conductivity cast aluminum alloy materials, alloying is required. US20190127824A1 discloses an Al-Mg-Si system motor rotor alloy, its preparation method, and its applications. By adding 0.3-0.5% Mg and 1-4.5% Si as the main alloying elements, controlling the impurity element Fe below 0.1%, and the grain-refining element TiB2 between 0.02-0.07%, a yield strength greater than 120 MPa and an electrical conductivity of 45-55% IACS are achieved. CN114635066A discloses an Al-Si-Fe system motor rotor alloy, its preparation method, and its applications. The aluminum alloy contains 0.2-0.4% Si, 0.1-0.3% Fe, and 0.2-1% Group IIA or IB elements (IIA: Mg; IB: Cu). This Al-Si-Fe system motor rotor alloy has a yield strength greater than 72 MPa and an electrical conductivity of 54-57% IACS. CN114875255A discloses a high-strength aluminum alloy for motor rotors and its preparation process. The high-strength aluminum alloy is obtained through elemental alloying with 0.5-1.5% Sb, 0.3-0.7% Mg, and 0.3-0.7% Si, exhibiting a yield strength greater than 80 MPa and an electrical conductivity of 55-59% IACS. CN114790527A discloses an Al-based ternary motor rotor alloy, its preparation method, and its applications. The alloying method includes 0.2-0.9 wt% Mg and 0.6-1.2 wt% Cu; or includes 0.2-0.9 wt% Mg and 1.5-2.5 wt% Zn; or includes 0.2-0.9 wt% Mg and 0.3-0.9 wt% Si. The final rotor alloy exhibits a yield strength greater than 60 MPa and an electrical conductivity greater than 53% IACS. CN114318085A discloses an aluminum alloy with excellent mechanical, electrical, and thermal conductivity properties and its manufacturing method. The aluminum alloy comprises 0.33-0.37% Si, 0.45-0.55% Mg, and 0.07-0.15% Fe, with the mass ratio of magnesium to silicon and one-third of iron being between 1.45 and 1.75. The alloy has a yield strength greater than 80 MPa and an electrical conductivity greater than 58% IACS. US2020 / 0407826 Al discloses an aluminum alloy comprising 0.2-3% Ce, 0.5-1.5% Si, 0.1-1.2% Fe, 0.2-1.0% Mg, Zn < 0.8%, Sr < 0.1%, Ti+Cr+Mn+V < 0.025%, with a yield strength greater than 115 MPa and an electrical conductivity greater than 45% IACS.
[0004] Most of the above technologies are based on the Al-Mg-Si system, using Mg2Si heat treatment to enhance the matrix strength while minimizing the impact on conductivity. Other alloy systems are then developed, such as doping with Sb and Ce to improve melt flowability and purity, respectively. A small number of alloys use Al2Cu heat treatment to strengthen the matrix. However, the individual strengthening effects of Mg2Si and Al2Cu are relatively poor, failing to balance the strength and conductivity of aluminum alloys.
[0005] Therefore, there is a need to develop an aluminum alloy material that combines high strength and high electrical conductivity. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide an aluminum alloy material, its preparation method, and its applications. This aluminum alloy material possesses the advantages of high strength and good electrical conductivity, making it suitable for manufacturing vehicle components such as motor rotors, stators, busbars, and inverters.
[0007] To achieve this objective, the present invention adopts the following technical solution:
[0008] In a first aspect, the present invention provides an aluminum alloy material, wherein the as-cast microstructure of the aluminum alloy material contains, in addition to the aluminum matrix, Mg2Si phase and Al2Cu phase.
[0009] The aluminum alloy material provided by this invention contains both Mg2Si phase and Al2Cu phase. By utilizing the strengthening effect of the two phases in combination, an aluminum alloy material with both high strength and high electrical conductivity is obtained.
[0010] In some embodiments of the present invention, the content of the Mg2Si phase is 0.2-1.4 wt%, and the content of the Al2Cu phase is 0.1-0.8 wt%. Through the combination of the Mg2Si and Al2Cu phases, the resulting aluminum alloy material exhibits an electrical conductivity ≥48% IACS, a yield strength ≥120 MPa at room temperature, a tensile strength ≥180 MPa, an elongation ≥10%, and a yield strength attenuation rate ≤10% after holding at 180℃ for 100 h.
[0011] The content of the Mg2Si phase can be 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, or 1.4wt%, etc.
[0012] The content of the Al2Cu phase can be 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, or 0.8wt%, etc.
[0013] In some embodiments of the present invention, the total content of the Mg2Si phase and the Al2Cu phase is 1.2-1.8 wt%, for example, it can be 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt%, 1.7 wt%, or 1.8 wt%, etc.
[0014] In this invention, if the content of Mg2Si phase and Al2Cu phase is too low, their strengthening effect is weak, which will lead to insufficient strength of aluminum alloy material; if the content of Mg2Si phase and Al2Cu phase is too high, it will rupture the matrix, resulting in a decrease in the elongation of aluminum alloy material.
[0015] In some embodiments of the present invention, the aluminum alloy material further contains a β-FeAlSi phase, or further contains Al. 15 (Fe,Mn)3Si2 phase and α-FeAlSi phase, or may also contain β-FeAlSi phase, Al 15 (Fe,Mn)3Si2 phase and α-FeAlSi phase.
[0016] In this invention, when the aluminum alloy material contains a certain amount of Fe, scrap aluminum with high iron content can be used as the raw material, which helps to reduce costs. When Mn is not added, Fe mainly exists as the β-FeAlSi phase, which is a needle-like phase; when Mn is added, it promotes the growth of Al... 15 The formation of (Fe,Mn)3Si2 phase and α-FeAlSi phase, which are in the shape of Chinese characters or in blocks, helps to improve the elongation of aluminum alloy materials.
[0017] In some embodiments of the present invention, the aluminum alloy material comprises the following components:
[0018] Si, Cu, Mg 0.3-1wt%, Fe≤0.5wt% and Mn≤0.15wt%, balance Al;
[0019] The contents of Si and Cu must satisfy the following conditions:
[0020]
[0021]
[0022] Among them, Mg and Si * The mass ratio is 1-2, Cu * The content is 0.2-0.6 wt%;
[0023] In Formulas 1 and 2, the element symbol represents the mass content of that element in the aluminum alloy.
[0024] This invention, through research, has discovered that when aluminum alloys simultaneously contain Si, Cu, and Mg elements, Al5Cu2Mg8Si6 impurity phases and / or Si phases may form, affecting the content of Mg2Si and Al2Cu phases. Therefore, the lower the content of Al5Cu2Mg8Si6 and Si phases, the better. Furthermore, when aluminum alloys also contain Fe and / or Mn, β-FeAlSi phases and / or Al... 15 The (Fe,Mn)3Si2 and α-FeAlSi phases consume some Si, affecting the content of the Mg2Si phase. Therefore, to ensure the formation of the desired amounts of Mg2Si and Al2Cu phases in the aluminum alloy, the content of each element needs to be controlled. This invention controls the content and proportion of each element to meet the above conditions, thereby ensuring that the content range of the Mg2Si and Al2Cu phases is within the range of this invention, resulting in an aluminum alloy material with both high strength and high electrical conductivity.
[0025] It should be noted that the Si described in this invention * This refers to the phase excluding β-FeAlSi and Al. 15 Si elements other than the (Fe,Mn)3Si2 phase and the α-FeAlSi phase; when the aluminum alloy does not contain Fe and Mn, Si * The content of Cu is equal to the content of Si. * It refers to Cu elements other than the Al5Cu2Mg8Si6 phase.
[0026] In this invention, the content of Mg is 0.3-1 wt%, for example, it can be 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, 0.5 wt%, 0.55 wt%, 0.6 wt%, 0.65 wt%, 0.7 wt%, 0.75 wt%, 0.8 wt%, 0.85 wt%, 0.9 wt%, or 1 wt%, etc.
[0027] The Fe content is ≤0.5wt%, for example, it can be 0.5wt%, 0.45wt%, 0.4wt%, 0.35wt%, 0.3wt%, 0.25wt%, 0.2wt%, 0.15wt%, 0.1wt%, 0.05wt%, or 0wt%. When the Fe content is 0.2-0.5wt%, the raw materials for preparing aluminum alloys, especially aluminum materials, can be either low-iron electrolytic aluminum or high-iron scrap aluminum. Aluminum alloys prepared using the latter as raw material not only have lower costs but also maintain or even exceed the performance of the former. When the Fe content is <0.2wt%, low-iron electrolytic aluminum can be used as raw material.
[0028] The content of Mn is ≤0.15wt%, for example, it can be 0.15wt%, 0.12wt%, 0.1wt%, 0.08wt%, 0.05wt%, 0.03wt%, or 0wt%, etc.
[0029] The Mg and Si * The mass ratio is 1-2, for example, it can be 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2, etc. If Mg and Si... * If the mass ratio is too large or too small, it can easily lead to an increase in the Al5Cu2Mg8Si6 phase and a decrease in the Mg2Si and Al2Cu phases, thereby reducing the electrical conductivity and strength of the aluminum alloy material.
[0030] The Cu * The content is 0.2-1wt%, for example, it can be 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, or 1wt%, etc.
[0031] In some embodiments of the present invention, the aluminum alloy material comprises the following components:
[0032] Si 0.3-1wt%, Cu 0.2-1wt%, Mg 0.3-1wt%, Fe≤0.5wt% and Mn≤0.15wt%, balance Al.
[0033] In some embodiments of the present invention, the content of Mg is 0.4-0.9 wt%.
[0034] In some embodiments of the present invention, the Mg and Si * The mass ratio is 1.4-1.8. When Mg and Si... * When the mass ratio is between 1.4 and 1.8, the precipitation strengthening effect of the Mg2Si phase is strongest.
[0035] In some embodiments of the present invention, the Fe content is 0.02-0.5 wt%.
[0036] In some embodiments of the present invention, the content of Mn is 0.05-0.15 wt%.
[0037] In some embodiments of the present invention, the aluminum alloy material further includes grain refining elements.
[0038] In some embodiments of the present invention, the content of the grain refining element is 0.01-0.1 wt%; for example, it may be 0.01 wt%, 0.02 wt%, 0.03 wt%, 0.04 wt%, 0.05 wt%, 0.06 wt%, 0.07 wt%, 0.08 wt%, 0.09 wt%, or 0.1 wt%.
[0039] In some embodiments of the present invention, the grain refining element is selected from one or more of Ti, Nb, V and Zr, preferably Ti.
[0040] Grain-refining elements help improve melt cleanliness, reduce hydrogen absorption tendency, and improve fluidity. They also refine α-Al grains, ultimately increasing the material's strength and elongation. In this invention, if the content of grain-refining elements is too low, their effects are difficult to achieve; if the content is too high, MAl3 (M = Ti, Nb, V, and / or Zr) impurities are easily generated. These impurities precipitate before α-Al and accumulate on the outer side under centrifugal force, leading to uneven local segregation and a decrease in the electrical conductivity, strength, and elongation of the aluminum alloy material.
[0041] In the aluminum alloy material of this invention, the impurity content is preferably ≤0.1wt%.
[0042] In a second aspect, the present invention provides a method for preparing an aluminum alloy material as described in the first aspect, the method comprising the following steps:
[0043] (1) According to the proportion of each element in the aluminum alloy material, the raw materials containing each element are mixed and smelted to obtain the first aluminum alloy liquid;
[0044] (2) The first aluminum alloy liquid is refined, degassed and slag removed to obtain the second aluminum alloy liquid;
[0045] (3) The second aluminum alloy liquid is kept at a certain temperature and then cast to obtain a casting;
[0046] (4) The casting is heat-treated to obtain the aluminum alloy material.
[0047] In some embodiments of the present invention, the melting temperature is 680-800℃ (e.g., it can be 680℃, 690℃, 700℃, 710℃, 720℃, 730℃, 740℃, 750℃, 760℃, 770℃, 780℃, 790℃ or 800℃, etc.), and the time is 120-180min (e.g., it can be 120min, 130min, 140min, 150min, 160min, 170min or 180min, etc.).
[0048] In some embodiments of the present invention, the refining temperature is 680-800℃ (e.g., it can be 680℃, 690℃, 700℃, 710℃, 720℃, 730℃, 740℃, 750℃, 760℃, 770℃, 780℃, 790℃, or 800℃, etc.), and the time is 15-30min (e.g., it can be 15min, 18min, 20min, 22min, 25min, 28min, or 30min, etc.).
[0049] In some embodiments of the present invention, the heat preservation temperature is 680-800℃ (e.g., it can be 680℃, 690℃, 700℃, 710℃, 720℃, 730℃, 740℃, 750℃, 760℃, 770℃, 780℃, 790℃ or 800℃, etc.), and the time is 30-120min (e.g., it can be 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min or 120min, etc.).
[0050] In some embodiments of the present invention, the casting is centrifugal casting.
[0051] In some embodiments of the present invention, the conditions for centrifugal casting are: mold preheating temperature of 650-730℃ (e.g., 650℃, 660℃, 670℃, 680℃, 690℃, 700℃, 710℃, 720℃, or 730℃, etc.), casting temperature of 710-750℃ (e.g., 710℃, 715℃, 720℃, 725℃, 730℃, 735℃, 740℃, 745℃, or 750℃, etc.), and demolding temperature of 300-400℃ (e.g., [missing information]). The temperature can be 300℃, 310℃, 320℃, 330℃, 340℃, 350℃, 360℃, 370℃, 380℃, 390℃, or 400℃, etc.), and the centrifugal speed can be 100-300r / min (e.g., 100r / min, 120r / min, 150r / min, 180r / min, 200r / min, 220r / min, 250r / min, 280r / min, or 300r / min, etc.), with the speed gradually decreasing during the casting process.
[0052] In some embodiments of the present invention, the heat treatment is performed as follows: first solution treatment, then water quenching, and then aging treatment. At this time, the solution treatment temperature is 500-550℃ (e.g., 500℃, 505℃, 510℃, 515℃, 520℃, 525℃, 530℃, 535℃, 540℃, 545℃, or 550℃, etc.), and the time is 4-10h (e.g., 4h, 5h, 6h, 7h, 8h, 9h, or 10h, etc.); the aging treatment temperature is 150-190℃ (e.g., 150℃, 155℃, 160℃, 165℃, 170℃, 175℃, 180℃, 185℃, or 190℃, etc.), and the time is 8-20h (e.g., 8h, 9h, 10h, 11h, 12h, 15h, 16h, 18h, or 20h, etc.).
[0053] In some embodiments of the present invention, the heat treatment is a direct aging process. In this case, the aging temperature is 180-300℃ (e.g., 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, 240℃, 250℃, 260℃, 270℃, 280℃, 290℃, or 300℃, etc.), and the time is 1-8 hours (e.g., 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, or 8 hours, etc.).
[0054] Generally, when the aging temperature is high, a shorter aging time should be selected; when the aging temperature is low, a longer aging time should be selected.
[0055] Thirdly, the present invention provides an application of the aluminum alloy material as described in the first aspect, wherein the aluminum alloy material is used to manufacture vehicle parts.
[0056] Preferably, the vehicle component is a motor rotor, wires, or an inverter.
[0057] Compared with the prior art, the present invention has the following beneficial effects:
[0058] This invention utilizes the strengthening effects of the Mg2Si phase and the Al2Cu phase to obtain an aluminum alloy material that combines high strength and high electrical conductivity.
[0059] Furthermore, through further optimization, the obtained aluminum alloy material has an electrical conductivity ≥48% IACS, a yield strength ≥120MPa at room temperature, a tensile strength ≥180MPa, an elongation ≥10%, and a yield strength attenuation rate ≤10% after holding at 180℃ for 100h. It can be used to cast vehicle parts such as motor rotors, motor stators, busbars, or inverters. Detailed Implementation
[0060] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the specific embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention.
[0061] Examples 1-18 and Comparative Examples 1-12
[0062] Examples 1-18 and Comparative Examples 1-12 each provide an aluminum alloy material, which is prepared according to the following method:
[0063] (1) According to the proportion of each element in the aluminum alloy material, industrial pure aluminum, Al-Si alloy, Al-Cu alloy, Al-Mg alloy, Al-Fe alloy, Al-Mn alloy, Al-Ti alloy, Al-Nb alloy, Al-V alloy and / or Al-Zr alloy are added to the melting furnace and melted at 740℃ for 120 min to obtain the first aluminum alloy liquid.
[0064] (2) Add 0.5wt% of refining agent to the first aluminum alloy liquid, refine at 740℃ for 15min, degas with high-purity argon, let stand for 15min and remove slag to obtain the second aluminum alloy liquid.
[0065] (3) The second aluminum alloy liquid was kept at 740°C for 30 minutes and the casting was prepared by centrifugal casting;
[0066] The conditions for centrifugal casting are as follows: mold preheating temperature is 720℃, casting temperature is 740℃, demolding temperature is 350℃, initial centrifugal speed is 250r / min, and the speed is gradually reduced to 0 during the casting process.
[0067] (4) The casting is first subjected to solution treatment, then water quenching, and then aging treatment, or directly subjected to aging treatment to obtain aluminum alloy material.
[0068] The content (wt%) of each element and the heat treatment conditions in the aluminum alloy materials provided in Examples 1-18 and Comparative Examples 1-12 are shown in Table 1 below:
[0069] Table 1. Element content (wt%) and heat treatment conditions
[0070]
[0071]
[0072] The proportions and microstructures of the elements in the aluminum alloy materials provided in Examples 1-18 and Comparative Examples 1-12 are shown in Table 2 below:
[0073] Table 2 Elemental Proportions and Organizational Information
[0074]
[0075]
[0076] The method for determining the content of Mg2Si and Al2Cu phases was as follows: Powder diffraction was performed on the powdered alloy sample using an X-ray diffractometer. The test conditions were: Cu target Kα rays; 2θ angle range 10–90°; scan step size 0.02°; scan speed 0.33° / s. The test results were then refined using Topas.
[0077] The method for testing the α-Al grain size is as follows: cut a cross section at a height of 20 mm from the bottom of the ingot (or at a uniform height), observe it with a polarizing metallographic microscope, and measure the average α-Al grain size using the cross section method (ASTM standard E112).
[0078] Performance testing:
[0079] The electrical conductivity, yield strength at room temperature, tensile strength, elongation, and high-temperature resistance of the aluminum alloy materials provided in Examples 1-18 and Comparative Examples 1-12 were tested using the following methods:
[0080] Electrical conductivity: Tested according to GB / T 12966-2022 Eddy current test method for electrical conductivity of aluminum and aluminum alloys;
[0081] Room temperature yield strength: Tested according to GB / T 228.1-2021 Metallic materials, tensile testing, Part 1: Room temperature test method;
[0082] Room temperature tensile strength: Tested according to GB / T 228.1-2021 Metallic materials, tensile testing, Part 1: Room temperature test method;
[0083] Room temperature elongation: Tested according to GB / T 228.1-2021 Metallic materials, tensile testing, Part 1: Room temperature test method;
[0084] High temperature resistance: The aluminum alloy material was kept at 180℃ for 100h, its yield strength was tested, and the strength decay rate was calculated.
[0085] The results of the above tests are shown in Table 3 below:
[0086] Table 3
[0087]
[0088]
[0089] As can be seen from the performance data of the above embodiments, the aluminum alloy material provided by the present invention has an electrical conductivity ≥48% IACS, a yield strength ≥120MPa at room temperature, a tensile strength ≥180MPa, an elongation ≥10%, and a yield strength attenuation rate ≤10% after being kept at 180℃ for 100h, thus possessing both high strength and high electrical conductivity.
[0090] Compared to Example 5, Comparative Example 1 had too low a Mg / Si* ratio, which led to an increase in the Al5Cu2Mg8Si6 content and a decrease in the Mg2Si and Al2Cu content, resulting in a decrease in the electrical conductivity and strength of the aluminum alloy material.
[0091] Compared to Example 6, Comparative Example 2 had an excessively high Mg / Si* ratio, which also led to an increase in the Al5Cu2Mg8Si6 content and a decrease in the Mg2Si and Al2Cu content, resulting in a decrease in the electrical conductivity and strength of the aluminum alloy material.
[0092] Compared with Example 1, the Cu in Comparative Example 3 * If the content is too low, the Al2Cu phase will be insufficient, resulting in a lack of reinforcing effect and a decrease in the strength and elongation of the aluminum alloy material.
[0093] Compared to Example 1, the Cu in Comparative Example 4 * Excessive content of Al2Cu phase leads to a decrease in the electrical conductivity and strength of aluminum alloy materials.
[0094] Compared with Example 1, Comparative Example 5 had too little Mg and Si content, and too little Mg2Si phase, resulting in insufficient reinforcing effect and a decrease in the strength of the aluminum alloy material.
[0095] Compared with Example 1, Comparative Example 6 had excessive Mg and Si content, and excessive Mg2Si phase, which led to a decrease in the electrical conductivity and strength of the aluminum alloy material.
[0096] Compared with Example 7, the solution treatment temperature in Comparative Example 7 was too low, resulting in insufficient solid dissolution of Mg, Si, and Cu elements, exacerbating lattice distortion, and consequently reducing the electrical conductivity and strength of the aluminum alloy material.
[0097] Compared with Example 8, the aging treatment temperature in Comparative Example 8 was too high and the time was too long, which led to an increase in the size of Mg2Si and Al2Cu, and consequently a decrease in the electrical conductivity and strength of the aluminum alloy material.
[0098] Compared with Example 18, the aging treatment temperature in Comparative Example 9 was too low and the time was too short, resulting in a low amount of Mg2Si and Al2Cu precipitation, and a decrease in the electrical conductivity and strength of the aluminum alloy material. Compared with Example 20, the aging treatment temperature in Comparative Example 10 was too high and the time was too long, resulting in an increase in the size of Mg2Si and Al2Cu, which in turn led to a decrease in the electrical conductivity and strength of the aluminum alloy material.
[0099] Compared with Example 1, Comparative Example 11 had an increased α-Al grain size and decreased strength and elongation in the aluminum alloy material because no grain refining elements were added; Comparative Example 12 had a large number of grain refining elements added, which led to the formation of TiAl3 impurity phase, resulting in a decrease in the electrical conductivity, strength and elongation of the aluminum alloy material.
[0100] The above description is merely a specific embodiment of this disclosure, enabling those skilled in the art to understand or implement it. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this disclosure. Therefore, this disclosure is not to be limited to the embodiments described herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An aluminum alloy material, characterized in that, In addition to the aluminum matrix, the as-cast microstructure of the aluminum alloy material also contains Mg2Si phase and Al2Cu phase, with the content of Mg2Si phase being 0.2-1.4 wt% and the content of Al2Cu phase being 0.1-0.8 wt%.
2. The aluminum alloy material according to claim 1, characterized in that, The total content of the Mg2Si phase and the Al2Cu phase is 1.2-1.8 wt%.
3. The aluminum alloy material according to claim 1 or 2, characterized in that, The aluminum alloy material also contains β-FeAlSi phase, or also contains Al 15 (Fe,Mn)3Si2 phase and α-FeAlSi phase, or may also contain β-FeAlSi phase, Al 15 (Fe,Mn)3Si2 phase and α-FeAlSi phase.
4. The aluminum alloy material according to claim 1 or 2, characterized in that, The aluminum alloy material comprises the following components: Si, Cu, Mg 0.3-1 wt%, Fe ≤0.5 wt%, and Mn ≤0.15 wt%, with the balance being Al; The contents of Si and Cu must satisfy the following conditions: Official 1; Official 2; Among them, Mg and Si The mass ratio is 1-2, Cu The content is 0.2-0.6 wt%; In Formulas 1 and 2, the element symbol represents the mass content of that element in the aluminum alloy.
5. The aluminum alloy material according to claim 4, characterized in that, The aluminum alloy material comprises the following components: Si 0.3-1 wt%, Cu 0.2-1 wt%, Mg 0.3-1 wt%, Fe ≤0.5 wt% and Mn ≤0.15 wt%, with the balance being Al.
6. The aluminum alloy material according to claim 4, characterized in that, The content of Mg is 0.4-0.9 wt%.
7. The aluminum alloy material according to claim 4, characterized in that, The Mg and Si The mass ratio is 1.4-1.
8.
8. The aluminum alloy material according to claim 4, characterized in that, The Fe content is 0.02-0.5 wt%.
9. The aluminum alloy material according to claim 4, characterized in that, The Mn content is 0.05-0.15 wt%.
10. The aluminum alloy material according to claim 4, characterized in that, The aluminum alloy material also includes grain-refining elements.
11. The aluminum alloy material according to claim 10, characterized in that, The content of the grain-refining element is 0.01-0.1 wt%.
12. The aluminum alloy material according to claim 10, characterized in that, The grain-refining element is selected from one or more of Ti, Nb, V and Zr.
13. A method for preparing an aluminum alloy material as described in any one of claims 1-12, characterized in that, The preparation method includes the following steps: (1) According to the proportion of each element in the aluminum alloy material, the raw materials containing each element are mixed and smelted to obtain the first aluminum alloy liquid; (2) The first aluminum alloy liquid is refined, degassed and deslag removed to obtain the second aluminum alloy liquid; (3) The second aluminum alloy liquid is kept at a certain temperature and then cast to obtain a casting; (4) The casting is heat-treated to obtain the aluminum alloy material.
14. The preparation method according to claim 13, characterized in that, The melting temperature is 680-800℃ and the time is 120-180min.
15. The preparation method according to claim 13, characterized in that, The refining temperature is 680-800℃ and the time is 15-30 minutes.
16. The preparation method according to claim 13, characterized in that, The insulation temperature is 680-800℃, and the time is 30-120 min.
17. The preparation method according to claim 13, characterized in that, The casting is centrifugal casting.
18. The preparation method according to claim 17, characterized in that, The conditions for centrifugal casting are as follows: mold preheating temperature 650-730℃, casting temperature 710-750℃, demolding temperature 300-400℃, centrifugal speed 100-300r / min, and the speed gradually decreasing during the casting process.
19. The preparation method according to claim 13, characterized in that, The heat treatment is as follows: first, solution treatment is performed, then water quenching is performed, and then aging treatment is performed; the solution treatment temperature is 500-550℃ and the time is 4-10h; the aging treatment temperature is 150-190℃ and the time is 8-20h.
20. The preparation method according to claim 13, characterized in that, The heat treatment is a direct aging process; the aging process is carried out at a temperature of 180-300℃ for a time of 1-8 hours.
21. An application of the aluminum alloy material as described in any one of claims 1-12, characterized in that, The aluminum alloy material is used to manufacture vehicle parts.
22. The application according to claim 21, characterized in that, The vehicle components are motor rotors, wires, or inverters.
Citation Information
Patent Citations
Aluminum alloy with excellent mechanical and electrical thermal conductivity and manufacturing method thereof
CN114318085A
Al-Si-Fe series motor rotor alloy and preparation method and application thereof
CN114635066A
Al-based ternary motor rotor alloy and preparation method and application thereof
CN114790527A
High-strength motor rotor aluminum alloy and preparation process thereof
CN114875255A
Casting aluminum alloys for high-performance applications
US20190127824A1