Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display assembly
By using amide compounds with specific structures and polymer liquid crystal alignment agents, a photoalignment film is formed, which solves the problem of flickering in liquid crystal display components and improves the performance of liquid crystal display components.
Patent Information
- Application Number
- CN202311235897.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-03
- Filing Date
- 2023-09-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-09-22
AI Technical Summary
The liquid crystal alignment films prepared by the existing photoalignment method are prone to flickering in liquid crystal display components, making it difficult to meet the requirements of high efficiency, high precision and large size.
A liquid crystal alignment film is formed by photoalignment using a liquid crystal alignment agent comprising an amide compound and a polymer with a specific structure. The specific structure of the liquid crystal alignment agent is that of the amide compound and polymer shown in formula (I), including polyamic acid polymer, polyimide polymer or their block copolymer.
The flicker of the liquid crystal display component was reduced, and the contrast and viewing angle characteristics of the liquid crystal display component were improved, meeting the requirements of high efficiency, high precision and large size.
Smart Images

Figure CN118011690B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a liquid crystal alignment agent, a liquid crystal alignment film, and a liquid crystal display component, particularly to a flicker-resistant liquid crystal alignment agent, a liquid crystal alignment film formed from the aforementioned liquid crystal alignment agent, and a liquid crystal display component having the aforementioned liquid crystal alignment film. Background Technology
[0002] Liquid crystal display components in LCD TVs, LCD monitors, etc., typically have a liquid crystal alignment film inside the component to control the alignment of the liquid crystals. Currently, the most common industrial method for forming liquid crystal alignment films is to form a film on an electrode substrate using polyamic acid and / or imidized polyimide, followed by a rubbing treatment (i.e., rubbing the film surface in a single direction with a cloth such as cotton, nylon, or polyester) to obtain the liquid crystal alignment film.
[0003] In the alignment process of liquid crystal alignment films, the easiest method to produce industrially is to perform a friction treatment on the film surface. However, with the increasing demands for high efficiency, high precision, and large size of liquid crystal display components, various problems such as damage to the liquid crystal alignment film surface, dust, the effects of mechanical and electrostatic forces, and non-uniformity on the alignment surface have become more pronounced during the friction treatment process.
[0004] As an alternative to friction treatment, photoalignment, which utilizes ultraviolet irradiation with polarized light to impart alignment energy to liquid crystals, is currently known. The liquid crystal alignment treatment in this photoalignment method can include substances that utilize photoisomerization, photocrosslinking, or photodecomposition reactions in their reaction mechanisms. Furthermore, Japanese Patent Application Publication No. 9-297313 proposes that the photoalignment method requires the use of a polyimide film with an alicyclic structure such as cyclobutane in its main chain. When using polyimide as the alignment film for photoalignment, its application is highly anticipated because this type of alignment film exhibits higher heat resistance than other types of alignment films.
[0005] Photoalignment is a method that does not require rubbing alignment. In industry, it not only has the advantage of simple process, but also, in liquid crystal display components driven by In-Plane-Switching (IPS) and Fringe Field Switching (FFS) technologies, compared with liquid crystal alignment films obtained by rubbing, the liquid crystal alignment film obtained by photoalignment is expected to improve the contrast and viewing angle characteristics of the liquid crystal display component. Therefore, photoalignment is a promising and highly regarded liquid crystal alignment method.
[0006] However, when liquid crystal alignment films prepared by photoalignment are applied to liquid crystal display components, flickering remains a problem. Therefore, in order to meet the requirements of current manufacturers of photoaligned IPS liquid crystal displays, providing a liquid crystal alignment agent for liquid crystal display components that is less prone to flickering (low flicker) has become the goal of research in this field. Summary of the Invention
[0007] This invention provides a liquid crystal alignment agent, comprising:
[0008] Polymer (A);
[0009] Solvent (B); and
[0010] An amide compound (C) comprising the structure shown in formula (I):
[0011]
[0012] In formula (I), L1 and L2 each independently represent alkyl groups having 1 to 10 carbon atoms;
[0013] Ra and Rb each independently represent alkyl groups having 1 to 6 carbon atoms; and
[0014] * indicates the junction.
[0015] The present invention also provides a liquid crystal alignment film formed from the aforementioned liquid crystal alignment agent.
[0016] The present invention also provides a liquid crystal display component comprising the aforementioned liquid crystal alignment film. Attached Figure Description
[0017] Figure 1 This is a side view of a liquid crystal display assembly according to an embodiment of the present invention.
[0018] 100: Liquid Crystal Display Components
[0019] 110: Unit 1
[0020] 112: First substrate
[0021] 114: First conductive film
[0022] 116: The first liquid crystal alignment film
[0023] 120: Unit Two
[0024] 122: Second substrate
[0025] 126: Second liquid crystal alignment film
[0026] 130: Liquid Crystal Unit Detailed Implementation
[0027] This invention provides a liquid crystal alignment agent, comprising:
[0028] Polymer (A);
[0029] Solvent (B); and
[0030] An amide compound (C) comprising the structure shown in formula (I):
[0031]
[0032] In formula (I), L1 and L2 each independently represent alkyl groups having 1 to 10 carbon atoms;
[0033] Ra and Rb each independently represent alkyl groups having 1 to 6 carbon atoms; and
[0034] * indicates the junction.
[0035] Polymer (A)
[0036] The polymer (A) of the present invention may comprise a first polymer (A1) and may optionally further comprise a second polymer (A2), as detailed below.
[0037] First polymer (A1)
[0038] The first polymer (A1) of the present invention is obtained by reacting a first mixture. Specifically, the first polymer (A1) may be selected from polyamic acid polymers, polyimide polymers, polyimide-based block copolymers, or any combination thereof. The polyimide-based block copolymer is selected from polyamic acid block copolymers, polyimide block copolymers, polyamic acid-polyimide block copolymers, or any combination thereof.
[0039] The first mixture comprises a tetracarboxylic dianhydride component (a1) and a diamine component (b1), wherein the tetracarboxylic dianhydride component (a1) includes at least one tetracarboxylic dianhydride compound (a1-1) represented by formula (III):
[0040]
[0041] In formula (II), R1, R2, R3 and R4 each independently represent a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group containing a fluorine atom and having 1 to 6 carbon atoms, or a phenyl group. R1, R2, R3 and R4 may be the same or different, and at least one of R1, R2, R3 and R4 is not a hydrogen atom.
[0042] When R1, R2, R3, and R4 have a steric barrier structure, the liquid crystal alignment of the liquid crystal alignment agent will be poor. Therefore, R1, R2, R3, and R4 are preferably hydrogen atoms, methyl groups, or ethyl groups, with methyl groups being more preferred.
[0043] Specific examples of the tetracarboxylic dianhydride compound (a1-1) with the structure shown in formula (II) are, for example, the compounds shown in formulas (II-1) to (II-8). Formula (II-1) is preferred for liquid crystal alignment.
[0044]
[0045]
[0046] The aforementioned tetracarboxylic acid dianhydride compound (a1-1) can be used alone or in combination.
[0047] Based on the total amount of tetracarboxylic dianhydride component (a1) being used in 100 moles, the amount of tetracarboxylic dianhydride compound (a1-1) being used can be from 10 moles to 80 moles; preferably from 10 moles to 70 moles; more preferably from 10 moles to 60 moles.
[0048] The tetracarboxylic dianhydride component (a1) may further include other tetracarboxylic dianhydride compounds (a1-2), preferred examples of which are (1) aliphatic tetracarboxylic dianhydride compounds, (2) alicyclic tetracarboxylic dianhydride compounds, (3) aromatic tetracarboxylic dianhydride compounds or (4) tetracarboxylic dianhydride compounds having the formulas (a1-2-1) to (a1-2-6).
[0049] The (1) aliphatic tetracarboxylic dianhydride compound includes, but is not limited to, aliphatic tetracarboxylic dianhydride compounds such as ethane tetracarboxylic dianhydride or butane tetracarboxylic dianhydride.
[0050] The alicyclic tetracarboxylic dianhydride compound (2) includes, but is not limited to, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dichloro-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1, Alicyclic tetracarboxylic anhydride compounds such as 2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 3,3',4,4'-dicyclohexyltetracarboxylic dianhydride, cis-3,7-dibutylcycloheptyl-1,5-diene-1,2,5,6-tetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, or bicyclo[2.2.2]-oct-7-ene-2,3,5,6-tetracarboxylic dianhydride.
[0051] Specific examples of the aromatic tetracarboxylic dianhydride compound (3) may include, but are not limited to, 3,4-dicarboxy-1,2,3,4-tetrahydronaphthalene-1-succinic dianhydride, benzopyrene tetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyl sulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 3,3'-4,4'-diphenylethane tetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic dianhydride, 1,2,3,4-furan tetracarboxylic dianhydride, and 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride. Carboxylic acid dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic acid dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, 2,3,3',4'-diphenyl sulfide tetracarboxylic acid dianhydride, 3,3',4,4'-diphenyl sulfide tetracarboxylic acid dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfone dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidene diphthalic acid dianhydride, 2,2',3,3'-diphenyltetracarboxylic acid dianhydride, 2,3,3',4'-diphenyltetracarboxylic acid dianhydride, 3,3',4,4'-diphenyltetracarboxylic acid dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-extrin-phenyl-bis(triphenylphthalic acid)di Anhydride, m-extrin-phenyl-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenyl ether dianhydride, bis(triphenylphthalic acid)-4,4'-diphenylmethane dianhydride, ethylene glycol-bis(dehydrated trimellitate), propylene glycol-bis(dehydrated trimellitate), 1,4-butanediol-bis(dehydrated trimellitate), 1,6-hexanediol-bis(dehydrated trimellitate), 1,8-octanediol-bis(dehydrated trimellitate), 2,2-bis(4-hydroxyphenyl)propane-bis(dehydrated trimellitate), 2,3,4,5-tetrahydrofuran tetracarboxylic acid dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-disideoxy-3-furanyl)-naphtho[1,2-c]-furan- 1,3-Diketone, 1,3,3a,4,5,9b-hexahydro-5-methyl-5-(tetrahydro-2,5-dioxy-3-furanyl)-naphtho[1,2-c]-furan-1,3-diketone, 1,3,3a,4,5,9b-hexahydro-5-ethyl-5-(tetrahydro-2,5-dioxy-3-furanyl)-naphtho[1,2-c]-furan-1,3-diketone, 1,3,3a,4,5,9b-hexahydro-7-methyl-5-(tetrahydro-2,5-dioxy-3-furanyl)-naphtho[1,2-c]-furan-1,3-diketone, 1,3,3a,4,5,9b-hexahydro-7-ethyl-5-(tetrahydro-2,5-dioxy-3-furanyl)-naphtho[1,[2-c]-furan-1,3-dione, 1,3,3a,4,5,9b-hexahydro-8-methyl-5-(tetrahydro-2,5-dioxy-3-furanyl)-naphtho[1,2-c]-furan-1,3-dione, 1,3,3a,4,5,9b-hexahydro-8-ethyl-5-(tetrahydro-2,5-dioxy-3-furanyl)-naphtho[1,2-c]-furan-1,3-dione, 1,3,3a,4,5,9b-hexahydro-5,8-dimethyl-5-(tetrahydro-2,5-dioxy-3-furanyl)-naphtho[1,2-c]-furan-1,3-dione, 5-(2,5-dioxytetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic acid dianhydride, etc.
[0052] The (4) comprises a tetracarboxylic acid dianhydride compound as shown in formulas (a1-2-1) to (a1-2-6), which is described in detail below:
[0053]
[0054]
[0055]
[0056] In formula (a1-2-5), A1 represents a divalent group containing an aromatic ring; r represents an integer from 1 to 2; A2 and A3 may be the same or different, and may represent a hydrogen atom or an alkyl group, respectively. Preferably, the tetracarboxylic dianhydride compound shown in formula (a1-2-5) is selected from the compounds shown in formulas (a1-2-51) to (a1-2-53).
[0057]
[0058] In formula (a1-2-6), A4 represents a divalent group containing an aromatic ring; A5 and A6 may be the same or different, and respectively represent a hydrogen atom or an alkyl group. Preferably, the tetracarboxylic dianhydride compound shown in formula (a1-2-6) may be selected from the compound shown in formula (a1-2-61).
[0059]
[0060] In the tetracarboxylic dianhydride component (a1), the aforementioned tetracarboxylic dianhydride compounds (a1-2) can be used alone or in combination.
[0061] The diamine component (b1) comprises at least one diamine compound (b1-1) selected from diamine compounds having the structure shown in formula [A-1], diamine compounds having the structure shown in formula [A-2], and diamine compounds having the structure shown in formula [A-3]:
[0062]
[0063] In formulas [A-1] to [A-3], R5 and R6 each independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a protecting group, and at least one of them is a protecting group; R7, R8, and R9 each independently represent a hydrogen atom, a monovalent hydrocarbon group having 1 to 20 carbon atoms, or a monovalent hydrocarbon group having 1 to 20 carbon atoms with a substituent; D represents a protecting group.
[0064] From the viewpoint of the storage stability of the liquid crystal alignment agent, the protecting group is preferably one that does not detach at room temperature, and more preferably one that detaches at 80°C or above, and more preferably at 100°C or above. The protecting group is preferably a group represented by the following formula (1) or a 9-fluorenylmethoxycarbonyl group.
[0065]
[0066] In formula (1), E represents a single bond or a divalent group containing a hydrocarbon group having 1 to 4 carbon atoms, preferably a divalent group containing an alkylene group. From the viewpoint of the removal temperature, tert-butoxycarbonyl (Boc) is preferred.
[0067] As a preferred example of a diamine compound having the structure shown in formula [A-1] above, diamine compounds as shown in formula [A-1-1] can be cited.
[0068]
[0069] In equation [A-1-1], R5 and R6 are the same as in equation [A-1], and also include their respective preferred examples. The two cs each independently represent an integer from 0 to 3, preferably 0 or 1, and more preferably 1.
[0070] In addition, in formula [A-1-1], the bonding position of the amino group (-NH2) in each benzene ring relative to the alkylene group can be any one of the ortho, meta, or para positions, preferably ortho or para, and more preferably para.
[0071] As preferred examples of diamine compounds represented by formula [A-1-1], the following compounds can be listed.
[0072]
[0073]
[0074] In formula [A-2], R7 and R8 each independently represent a hydrogen atom, a monovalent hydrocarbon group having 1 to 20 carbon atoms, or a monovalent hydrocarbon group having 1 to 20 carbon atoms with substituents. Preferably, they are hydrogen atoms, alkyl groups having 1 to 6 carbon atoms, or phenyl groups; more preferably, they are hydrogen atoms or methyl groups.
[0075] D represents a protecting group, including its preferred examples, as defined in formula [A-2] above, and more preferably a tert-butoxycarbonyl group.
[0076] The diamine compound having the structure shown in formula [A-2] is preferably the diamine compound shown in formula [A-2-1].
[0077]
[0078] More preferably, it is a diamine compound represented by formula [A-2-2].
[0079]
[0080] A 1 and A 5 Each independently represents a single bond or an alkylene group having 1 to 5 carbon atoms. A single bond or a methylene group is preferred. 2 and A 4 Represents an alkylene group having 1 to 5 carbon atoms, preferably methylene or ethylene.
[0081] A 3 Represents an alkylene or cycloalkylene group having 1 to 6 carbon atoms, preferably a methylene or ethylene group.
[0082] B 1 and B 2 Each can independently represent a single bond, -O-, -NH-, -NMe-, -C(=O)-, -C(=O)O-, -C(=O)NH-, -C(=O)NMe-, -OC(=O)-, -NHC(=O)-, or -N(Me)C(=O)-. A single bond or -O- is preferred.
[0083] D1 represents tert-butoxycarbonyl or 9-fluorenylmethoxycarbonyl. From the viewpoint of the deprotection temperature, tert-butoxycarbonyl is preferred.
[0084] a is 0 or 1.
[0085] As specific examples of the diamine represented by formula [A-2-2], formulas (2-1) to (2-21) can be listed below.
[0086]
[0087]
[0088]
[0089] In formulas (2-1) to (2-21), Me represents methyl and D2 represents tert-butoxycarbonyl.
[0090] Among them, equations (2-1) to (2-4) are preferred, and equation (2-1) is even more preferred.
[0091] The diamine compound having the structure shown in formula [A-3] is preferably the one shown in formula [A-3-1] or formula [A-3-2].
[0092]
[0093] The preferred forms are shown in equations [A-3-3] and [A-3-4].
[0094]
[0095] In equations [A-3-1] and [A-3-3], A 1 A 5 A 2 B 1 and B 2 With A in equation [A-2-1] 1 A 5 A 2 B 1 and B 2 The same applies, including their respective preferred examples. R9 each independently represents a hydrogen atom, a monovalent hydrocarbon group having 1 to 20 carbon atoms, or a monovalent hydrocarbon group having 1 to 20 carbon atoms with substituents. From the viewpoint of liquid crystal orientation, R9 is preferably a hydrogen atom, a methyl or ethyl group, and more preferably a hydrogen atom.
[0096] A 6 The single bond represents an alkylene group having 1 to 6 carbon atoms, preferably a single bond, methylene, ethylene, or propylene, and more preferably a single bond or methylene.
[0097] D1 is either tert-butoxycarbonyl or 9-fluorenylmethoxycarbonyl, and from the viewpoint of the deprotection temperature, tert-butoxycarbonyl is preferred.
[0098] a is 0 or 1.
[0099] In equations [A-3-3] and [A-3-4], A 6 R9 and D1 are related to A in equations [A-3-1] and [A-3-3]. 6 R9 and D1 are the same, and also include their respective best examples.
[0100] As specific examples, equations (3-1) to (3-5) can be listed.
[0101]
[0102] In formulas (3-1) to (3-5), D2 is tert-butoxycarbonyl.
[0103] Among them, equations (3-1) to (3-4) are more preferred, and equation (3-1) is even more preferred.
[0104] The aforementioned diamine compound (b1-1) can be used alone or in combination.
[0105] Based on the total amount of diamine component (b1) used being 100 moles, the amount of the diamine compound (b1-1) used can be from 0.1 moles to 30 moles; preferably from 0.5 moles to 30 moles; more preferably from 0.5 moles to 25 moles.
[0106] When the diamine component (b) contains a diamine compound (b1-1), the resulting liquid crystal alignment agent has a lower scintillation level.
[0107] The diamine component (b1) may further comprise other diamine compounds (b1-2), which may include, but are not limited to, 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 4,4'-diaminoheptane, 1,3-diamino-2,2-dimethylpropane, 1,6-diamino-2,5-dimethylhexane, 1,7-diamino-2,5-dimethylheptane, 1,7-diamino-4,4-dimethylheptane, 1,7-diamino-3-methylheptane, and 1,9-diamino... -5-Methylnonane, 2,11-diaminododecane, 1,12-diaminooctadecane, 1,2-bis(3-aminopropoxy)ethane, 4,4'-diaminodicyclohexylmethane, 4,4'-diamino-3,3'-dimethyldicyclohexylamine, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, isophorone diamine, tetrahydrodicyclopentadiene diamine, tricyclo(6·2·1·02,7)-undecenedimethyldiamine, 4,4'-methylenebis(cyclohexylamine), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminobenzoylaniline, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl Ethers, 1,5-diaminonaphthalene, 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylhydroindene, 6-amino-1-(4'-aminophenyl)-1,3,3-trimethylhydroindene, hexahydro-4,7-methyl-bridged indene dimethylenediamine, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 4,4'-diaminobenzophenone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]sulfone, 1,4-bis(4-aminophenoxy)cyclohexane, 1,5-bis(4-aminophenyl) (Oxymethyl)adamantane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 9,9-bis(4-aminophenyl)-10-hydroanthracene, 9,10-bis(4-aminophenyl)anthracene, 2,7-diaminophen, 9,9-bis(4-aminophenyl)phen, 4,4'-methylene-bis(2-chloroaniline), 4,4'-(p-epylphenylisopropylidene)bisaniline, 4,4'-(m-epylphenylisopropylidene)bisaniline, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, 4,4'-bis[(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl, 5-[4-(4-n-pentylcyclohexyl)cyclohexyl]phenylmethylene-1,3-diaminobenzene, 1,1-bis[4-(4-aminophenoxy)phenyl]-4-(4-ethylphenyl)cyclohexane phenyl)cyclohexane, 3,5-diaminobenzoic acid, 2,5-diaminobenzoic acid, bis(4-aminophenoxy)methane, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,3-bis(3-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,4-bis(3-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,5-bis(3-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 1,6-bis(3-aminophenoxy)hexane, 1,7-bis(4-aminophenoxy)heptane 1,7-bis(3-aminophenoxy)heptane, 1,8-bis(4-aminophenoxy)octane, 1,8-bis(3-aminophenoxy)octane, 1,9-bis(4-aminophenoxy)nonane, 1,9-bis(3-aminophenoxy)nonane, 1,10-bis(4-aminophenoxy)decane, 1,10-bis(3-aminophenoxy)decane, 1,11-bis(4-aminophenoxy)undecane, 1,11-bis(3-aminophenoxy)undecane, 1,12-bis(4-aminophenoxy)dodecane, 1,12-bis(3-aminophenoxy)dodecane, or other diamine compounds as shown in formulas (b-1) to (b-29).
[0108] Equation (b-1) is shown below:
[0109]
[0110] In equation (b-1), Z1 represents Z2 represents a monovalent group containing a steroidal group, trifluoromethyl group, fluorine group, alkyl group with 2 to 30 carbon atoms, or a nitrogen-containing cyclic structure derived from pyridine, pyrimidine, triazine, piperidine, and piperazine.
[0111] The other diamine compounds shown in formula (b-1) above are preferably 2,4-diaminophenyl ethyl formate, 3,5-diaminophenyl ethylformate, 2,4-diaminophenyl propyl formate, 3,5-diaminophenyl propyl formate, 1-dodecoxy-2,4-diaminobenzene, 1-hexadecoxy-2,4-diaminobenzene, 1-octadecoxy-2,4-diaminobenzene, or other diamine compounds shown in formulas (b-1-1) to (b-1-6).
[0112]
[0113]
[0114] Equation (b-2) is shown below:
[0115]
[0116] In equation (b-2), Z3 represents Z4 and Z5 represent aliphatic rings, aromatic rings, or heterocyclic groups, and Z6 represents an alkyl group having 3 to 18 carbon atoms, an alkoxy group having 3 to 18 carbon atoms, a fluoroalkyl group having 1 to 5 carbon atoms, a fluoroalkoxy group having 1 to 5 carbon atoms, a cyano group, or a halogen atom.
[0117] Other diamine compounds shown in formula (b-2) above are preferably diamine compounds shown in formulas (b-2-1) to (b-2-13) below:
[0118]
[0119]
[0120]
[0121] In equations (b-2-10) to (b-2-13), s can represent an integer from 3 to 12.
[0122] Equation (b-3) is shown below:
[0123]
[0124] In formula (b-3), Z7 represents a hydrogen atom, an acyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen. P1 represents an integer from 1 to 3. When P1 is greater than 1, multiple Z7s can be the same or different.
[0125] The diamine compound shown in formula (b-3) above is preferably selected from (1) p-diaminebenzene, m-diaminebenzene, o-diaminebenzene or 2,5-diaminetoluene when P1 is 1; (2) 4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 2,2'-dichloro-4,4'-diaminobiphenyl, 3,3'-dichloro-4,4'-diaminobiphenyl when P1 is 2. Benzene, 2,2',5,5'-tetrachloro-4,4'-diaminobiphenyl, 2,2'-dichloro-4,4'-diamino-5,5'-dimethoxybiphenyl or 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, etc.; (3) 1,4-bis(4'-aminophenyl)benzene when P1 is 3, preferably selected from p-diaminobenzene, 2,5-diaminotoluene, 4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl or 1,4-bis(4'-aminophenyl)benzene.
[0126] Equation (b-4) is shown below:
[0127]
[0128] In formula (b-4) above, P2 represents an integer from 1 to 5. The structure shown in formula (b-4) is preferably selected from 4,4'-diaminodiphenyl sulfide.
[0129] Equation (b-5) is shown below:
[0130]
[0131] In equation (b-5), Z8 and Z 10 They can be the same or different, and each represents a divalent organic group. Z9 represents a divalent group derived from nitrogen-containing cyclic structures such as pyridine, pyrimidine, triazine, piperidine, and piperazine.
[0132] Equation (b-6) is shown below:
[0133]
[0134] In equation (b-6), Z 11 Z 12 Z 13and Z 14 They can be the same or different, and can represent hydrocarbon groups with 1 to 12 carbon atoms. P3 represents an integer from 1 to 3, and P4 represents an integer from 1 to 20.
[0135]
[0136] In equation (b-7), Z 15 Represents -O- or cyclohexyl, Z 16 Representative: CH2-, Z 17 Represents phenyl or cyclohexyl, and Z 18 It represents a hydrogen atom or a heptyl group.
[0137] The diamine compound shown in formula (b-7) is preferably selected from the diamine compounds shown in formulas (b-7-1) and (b-7-2) below.
[0138]
[0139] Other diamine compounds represented by formulas (b-8) to (b-29) are shown below:
[0140]
[0141]
[0142]
[0143]
[0144]
[0145] In equations (b-16) to (b-19), Z 19 Preferably selected from alkyl groups having 1 to 10 carbon atoms or alkoxy groups having 1 to 10 carbon atoms. In formulas (b-20) to (b-24), Z 20 Preferably, it is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms.
[0146] Other diamine compounds (b1-2) preferably include, but are not limited to, 1,2-diaminoethane, 4,4'-diaminodicyclohexylmethane, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 5-[4-(4-n-pentylcyclohexyl)cyclohexyl]phenylmethylene-1,3-diaminobenzene, 1,3-bis(3-aminophenoxy)benzene, and 1,1-bis[4-(4-aminophenoxy)phenyl]-4-(4-ethyl Compounds represented by (b-2,4-diaminophenyl)cyclohexane, ethyl 2,4-diaminophenylformate, p-diaminebenzene, m-diaminebenzene, o-diaminebenzene, 1,2-bis(4-aminophenoxy)ethane, 1,5-bis(4-aminophenoxy)pentane, and compounds represented by formula (b-1-1), (b-1-2), (b-1-5), (b-2-1), (b-2-11), (b-7-1), (b-25), or (b-28).
[0147] The other diamine compounds (b1-2) mentioned above can be used alone or in combination.
[0148] Preparation method of the first polymer (A1)
[0149] The preparation of the polyamic acid polymer in this invention can be carried out by a general method. Preferably, the preparation method of the aforementioned polyamic acid polymer includes the following steps: dissolving a first mixture containing a tetracarboxylic acid dianhydride component (a1) and a diamine component (b1) in a solvent, carrying out a polycondensation reaction at a temperature of 0°C to 100°C for 1 to 24 hours, and then performing vacuum distillation on the above reaction solution in an evaporator to obtain the polyamic acid polymer, or pouring the above reaction solution into a large amount of lean solvent to obtain a precipitate, and then drying the precipitate by vacuum drying to obtain the polyamic acid polymer.
[0150] The solvent used in the polycondensation reaction may be the same as or different from the solvent in the liquid crystal alignment agent described below, and there are no particular limitations on the solvent used in the polycondensation reaction, as long as it can dissolve the reactants and products. Preferably, the solvent includes, but is not limited to, (1) aprotic polar solvents, such as: N-methyl-2-pyrrolidinone (NMP), N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, tetramethylurea or hexamethylphosphonic triamine, etc.; (2) phenolic solvents, such as: m-cresol, xylenol, phenol or halogenated phenols, etc. Based on the amount of the mixture used being 100 parts by weight, the amount of solvent used in the polycondensation reaction is preferably from 200 parts by weight to 2000 parts by weight, more preferably from 300 parts by weight to 1800 parts by weight.
[0151] In particular, in polycondensation reactions, solvents can be used in combination with appropriate amounts of lean solvents, where the lean solvents do not cause the polyamic acid polymer to precipitate. Lean solvents can be used alone or in combination, and include, but are not limited to, (1) alcohols, such as methanol, ethanol, isopropanol, cyclohexanol, ethylene glycol, propylene glycol, 1,4-butanediol, or triethylene glycol; (2) ketones, such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.; (3) esters, such as methyl acetate, ethyl acetate, butyl acetate, diethyl oxalate, diethyl malonate, or ethylene glycol ethyl ether acetate, etc.; (4) ethers. For example: ethers such as diethyl ether, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol n-propyl ether, ethylene glycol isopropyl ether, ethylene glycol n-butyl ether, ethylene glycol dimethyl ether or diethylene glycol dimethyl ether; (5) halogenated hydrocarbons, such as: dichloromethane, 1,2-dichloroethane, 1,4-dichlorobutane, trichloroethane, chlorobenzene or o-dichlorobenzene; (6) hydrocarbons, such as: tetrahydrofuran, hexane, heptane, octane, benzene, toluene or xylene or any combination of the above solvents. Based on the use of 100 parts by weight of diamine component (b1), the use of lean solvent is preferably 0 to 60 parts by weight, more preferably 0 to 50 parts by weight.
[0152] The preparation of the polyimide polymer in this invention can be carried out using a general method. Preferably, the method involves first dissolving a first mixture in a solution, wherein the first mixture contains a tetracarboxylic acid dianhydride component (a1) and a diamine component (b1), and then performing a polymerization reaction to form a polyamic acid polymer. Next, in the presence of a dehydrating agent and a catalyst, the mixture is further heated, and a dehydration dead-cycle reaction is carried out, causing the amic acid functional groups in the polyamic acid polymer to be converted into imide functional groups (i.e., imidization) through the dehydration dead-cycle reaction, thereby obtaining the polyimide polymer.
[0153] The solvent used in the dehydration dead-cycle reaction can be the same as the solvent in the liquid crystal alignment agent described below, and therefore will not be described again. Based on the amount of polyamic acid polymer used being 100 parts by weight, the amount of solvent used in the dehydration dead-cycle reaction is preferably 200 to 2000 parts by weight, more preferably 300 to 1800 parts by weight.
[0154] To obtain a better degree of imidization of the polyamic acid polymer, the operating temperature of the dehydration dead-cycle reaction is preferably between 40°C and 200°C, more preferably between 40°C and 150°C. If the operating temperature of the dehydration dead-cycle reaction is below 40°C, the imidization reaction will be incomplete, thus reducing the degree of imidization of the polyamic acid polymer. However, if the operating temperature of the dehydration dead-cycle reaction is above 200°C, the weight average molecular weight of the resulting polyimide polymer will be lower.
[0155] The dehydrating agent used in the dehydration dead-cycle reaction can be selected from acid anhydride compounds, specifically, acetic anhydride, propionic anhydride, or trifluoroacetic anhydride. Based on 1 mole of polyamic acid polymer, the amount of dehydrating agent used is 0.01 mole to 20 moles. The catalyst used in the dehydration dead-cycle reaction can be selected from (1) pyridine compounds, such as pyridine, trimethylpyridine, or dimethylpyridine; and (2) tertiary amine compounds, such as triethylamine. Based on 1 mole of dehydrating agent, the amount of catalyst used is 0.5 moles to 10 moles.
[0156] Preferred examples of the polyimide-based block copolymers of the present invention are polyamic acid block copolymers, polyimide block copolymers, polyamic acid-polyimide block copolymers, or any combination thereof.
[0157] The preparation of the polyimide-based block copolymer in this invention can be carried out by a general method. Preferably, the preparation method of the polyimide-based block copolymer is to first dissolve the starting material in a solvent and carry out a polycondensation reaction, wherein the starting material includes at least one polyamic acid polymer and / or at least one polyimide polymer mentioned above, and may further include a tetracarboxylic dianhydride component (a1) and a diamine component (b1).
[0158] The tetracarboxylic dianhydride component (a1) and diamine component (b1) in the aforementioned starting material are the same substances as those used in the preparation of polyamic acid polymers. Furthermore, the solvent used in the polycondensation reaction can be the same as the solvent in the liquid crystal alignment agent described below, which will not be elaborated further here.
[0159] Based on the aforementioned starting material being used in an amount of 100 parts by weight, the amount of solvent used in the polycondensation reaction is preferably from 200 parts by weight to 2000 parts by weight, more preferably from 300 parts by weight to 1800 parts by weight. The operating temperature of the polycondensation reaction is preferably from 0°C to 200°C, and more preferably from 0°C to 100°C.
[0160] Preferably, the starting material comprises, but is not limited to, (1) two polyamic acid polymers with different end groups and different structures; (2) two polyimide polymers with different end groups and different structures; (3) a polyamic acid polymer and a polyimide polymer with different end groups and different structures; (4) a polyamic acid polymer, a tetracarboxylic dianhydride compound, and a diamine compound, wherein at least one of the tetracarboxylic dianhydride compound and the diamine compound has a different structure from the tetracarboxylic dianhydride component (a1) and the diamine component (b1) used to form the polyamic acid polymer; (5) a polyimide polymer, a tetracarboxylic dianhydride compound, and a diamine compound, wherein at least one of the tetracarboxylic dianhydride compound and the diamine compound has a different structure from the tetracarboxylic dianhydride component (a1) and the diamine component (b1) used to form the polyimide polymer; and (6) a polyamic acid polymer and a polyimide polymer. (7) Two polyamic acid polymers, a tetracarboxylic acid dianhydride compound and a diamine compound, wherein at least one of the tetracarboxylic acid dianhydride compound and the diamine compound has a different structure from the tetracarboxylic acid dianhydride component (a1) and the diamine component (b1) used to form the polyamic acid polymer or the polyimide polymer; (8) Two polyimide polymers, a tetracarboxylic acid dianhydride compound and a diamine compound with different structures; (9) Two polyamic acid polymers with anhydride end groups and different structures and a diamine compound; (10) Two polyamic acid polymers with amine end groups and different structures and a tetracarboxylic acid dianhydride compound; (11) Two polyimide polymers with anhydride end groups and different structures and a diamine compound; (12) Two polyimide polymers with amine end groups and different structures and a tetracarboxylic acid dianhydride compound.
[0161] Preferably, without affecting the effectiveness of the present invention, the aforementioned polyamic acid polymer, the aforementioned polyimide polymer, and the aforementioned polyimide-based block copolymer can be end-modified polymers after prior molecular weight adjustment. By using end-modified polymers, the coating performance of the liquid crystal alignment agent can be improved. The aforementioned end-modified polymers can be prepared by adding a monofunctional compound during the polycondensation reaction of the polyamic acid polymer. The monofunctional compound includes, but is not limited to, (1) monocarboxylic anhydrides, such as maleic anhydride, phthalic anhydride, itaconic anhydride, n-decyl succinic anhydride, n-dodecyl succinic anhydride, n-tetradecyl succinic anhydride or n-hexadecyl succinic anhydride; (2) monoamine compounds, such as aniline, cyclohexylamine, n-butylamine, n-pentylamine, n-hexylamine, n-heptylamine, n-octylamine, n-nonylamine, n-decylamine, n-undecaneamine, n-dodecaneamine, n-tridecaneamine, n-tetradecaneamine, n-pentadecananeamine, n-hexadecaneamine, n-heptadecaneamine, n-octadecaneamine or n-eicosylamine; (3) monoisocyanate compounds, such as phenyl isocyanate or naphthyl isocyanate.
[0162] The first polymer (A1) of the present invention has a weight-average molecular weight of 10,000 to 100,000, more preferably 12,000 to 90,000, and even more preferably 12,000 to 75,000, as determined by gel permeation chromatography.
[0163] Second polymer (A2)
[0164] The second polymer (A2) of the present invention is obtained by reacting a second mixture. Specifically, the second polymer (A2) may be selected from polyamic acid polymers, polyimide polymers, polyimide-based block copolymers, or any combination thereof. The polyimide-based block copolymer is selected from polyamic acid block copolymers, polyimide block copolymers, polyamic acid-polyimide block copolymers, or any combination thereof.
[0165] The second mixture comprises a tetracarboxylic dianhydride component (a2) and a diamine component (b2), wherein the tetracarboxylic dianhydride component (a2) is the same as the other tetracarboxylic dianhydride compounds (a1-2) listed in the aforementioned first polymer (A1) tetracarboxylic dianhydride component (a1), and the diamine component (b2) is the same as the other diamine compounds (b1-2) listed in the aforementioned first polymer (A1) diamine component (b1), and therefore will not be described further here.
[0166] Preparation method of the second polymer (A2)
[0167] The preparation method of the second polymer (A2) of the present invention is the same as that of the first polymer (A1) described above. The difference is that the second polymer (A2) is prepared by reacting the aforementioned tetracarboxylic acid dianhydride component (a2) and diamine component (b2). Therefore, the preparation method of the second polymer (A2) will not be described again here.
[0168] The second polymer (A2) of the present invention has a weight-average molecular weight of 10,000 to 100,000, more preferably 12,000 to 90,000, and even more preferably 12,000 to 75,000, as determined by gel permeation chromatography.
[0169] The total amount of polymer (A) used is 100 parts by weight, the amount of the first polymer (A1) used is 5 parts by weight to 85 parts by weight, preferably 10 parts by weight to 80 parts by weight, more preferably 10 parts by weight to 75 parts by weight; the amount of the second polymer (A2) used is 15 parts by weight to 95 parts by weight, preferably 20 parts by weight to 90 parts by weight, more preferably 25 parts by weight to 90 parts by weight.
[0170] When the amounts of the first polymer (A1) and the second polymer (A2) used are within the aforementioned ranges, the resulting liquid crystal alignment agent exhibits a lower scintillation rate.
[0171] Solvent (B)
[0172] The solvent used in the liquid crystal alignment agent of the present invention is not particularly limited, as long as it can dissolve the polymer (A) and any other component without reacting with them. Preferably, it is the same solvent used in the synthesis of polyamic acid mentioned above. At the same time, the lean solvent used in the synthesis of polyamic acid mentioned above can also be used.
[0173] Specific examples of solvent (B) include, but are not limited to, N-methyl-2-pyrrolidone (NMP), γ-butyrolactone, γ-butyrolactam, 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monomethyl ether, butyl lactate, butyl acetate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol n-propyl ether, ethylene glycol isopropyl ether, ethylene glycol n-butyl ether, ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, or N,N-dimethylformamide or N,N-dimethylacetamide.
[0174] Solvent (B) can be used alone or in combination.
[0175] The amount of polymer (A) used is 100 parts by weight, and the amount of solvent (B) used is 800 parts by weight to 300 parts by weight, preferably 900 parts by weight to 3500 parts by weight, and even more preferably 1000 to 3000 parts by weight.
[0176] Amide compound (C)
[0177] The amide compound (C) of the present invention comprises the structure shown in formula (I):
[0178]
[0179] In formula (I), L1 and L2 each independently represent alkyl groups having 1 to 10 carbon atoms;
[0180] Ra and Rb each independently represent alkyl groups having 1 to 6 carbon atoms; and
[0181] * indicates the junction.
[0182] Preferably, Ra and Rb can be straight-chain alkyl groups having 1 to 6 carbon atoms, or branched alkyl groups having 3 to 6 carbon atoms. Examples of straight-chain alkyl groups having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, n-butyl, n-pentyl, and n-hexyl; examples of branched alkyl groups having 3 to 6 carbon atoms include isopropyl, isobutyl, dibutyl, tributyl, isopentyl, and isohexyl. More preferably, Ra and Rb being straight-chain alkyl groups having 1 to 6 carbon atoms results in a lower scintillation rate in the formed liquid crystal alignment agent.
[0183] The amide compound (C) of the present invention may comprise one or more structures shown in formula (I). For example, the structure of the amide compound (C) may be shown in formula (I-1) below:
[0184]
[0185] In formula (I-1), A represents an aliphatic hydrocarbon group with 1 to 20 carbon atoms, an alicyclic group with 3 to 30 carbon atoms, an aromatic hydrocarbon group with 6 to 30 carbon atoms, or a heterocyclic group with 6 to 30 carbon atoms. Preferably, A may be an alkyl group with 1 to 10 carbon atoms, an alicyclic group with 3 to 25 carbon atoms, an aromatic hydrocarbon group with 6 to 25 carbon atoms, or a heterocyclic group with 6 to 25 carbon atoms.
[0186] Furthermore, the definitions of L1, L2, L3, and L4 in formula (I-1) are the same as those of L1 and L2 in formula (I) above, and the definitions of Ra, Rb, Rc, and Rd in formula (I-1) are the same as those of Ra and Rb in formula (I) above, so they will not be repeated here. Preferably, Ra, Rb, Rc, and Rd are straight-chain alkyl groups with 1 to 6 carbon atoms, which can result in a lower scintillation of the formed liquid crystal alignment agent.
[0187] Amide compounds (C) can be listed as examples of the following formulas (I-1-1) to (I-1-9):
[0188]
[0189]
[0190]
[0191] Preparation method of amide compound (C)
[0192] The amide compound (C) of the present invention can be obtained by esterification of a polyol compound (C1) and a carboxylic acid compound (C2). The polyol compound (C1) is shown in the following formula (I-2):
[0193]
[0194] The definitions of A, L1, L2, L3, and L4 in equation (I-2) are the same as those in the aforementioned equation (I-1), so they will not be repeated here.
[0195] Examples of such polyol compounds (C1) are shown in the following formulas (I-2-1) to (I-2-9):
[0196]
[0197]
[0198] Examples of the carboxylic acid compound (C2) include acetic acid, propionic acid, n-butyric acid, n-valeric acid, n-hexanoic acid, n-heptanoic acid, isobutyric acid, 3-methylbutyric acid, and 4-methylvaleric acid (isohexanoic acid); acetic acid, n-propionic acid, n-butyric acid, and n-valeric acid are preferred; acetic acid and n-propionic acid are even more preferred. When an amide compound (C) synthesized from acetic acid, n-propionic acid, n-butyric acid, n-valeric acid, n-hexanoic acid, or n-heptanoic acid is used, the resulting liquid crystal alignment agent exhibits lower scintillation.
[0199] Examples of the aforementioned esterification reactions include: the reaction of carboxylic acids with acyl chlorides and alcohols to form esters; the reaction of acid anhydrides with alcohols to form esters; the reaction of carboxylic acids with carboxylate salts and haloalkanes to form esters; Fischer esterification; Steglich esterification; and Yamaguchi esterification; among which Steglich esterification is preferred.
[0200] The total amount of polymer (A) used is 100 parts by weight, and the amount of amide compound (C) used is 1 to 20 parts by weight, preferably 3 to 18 parts by weight, and more preferably 5 to 15 parts by weight.
[0201] When no amide compound (C) is used, the resulting liquid crystal alignment agent has a high scintillation rate.
[0202] Additive (D)
[0203] Without affecting the effectiveness of the present invention, the liquid crystal alignment agent of the present invention may selectively include an additive (D), and the additive (D) may be an epoxy compound or a silane compound having functional groups, etc. The function of the additive (D) is to improve the adhesion between the aforementioned liquid crystal alignment film and the substrate surface. The additive (D) may be used alone or in combination.
[0204] The aforementioned epoxy compounds may include, but are not limited to, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerol diglycidyl ether, 2,2-dibromonepentyl glycol diglycidyl ether, 1,3,5,6-tetracyclooxypropyl-2,4-hexanediol, N,N N',N'-Tetracyclooxypropyl-m-xylenediamine, 1,3-bis(N,N-dicyclooxypropylaminomethyl)cyclohexane, N,N,N',N'-tetracyclooxypropyl-4,4'-diaminodiphenylmethane, N,N-epoxypropyl-p-epoxypropoxyaniline, 3-(N-allyl-N-epoxypropyl)aminopropyltrimethoxysilane, 3-(N,N-dicyclooxypropyl)aminopropyltrimethoxysilane, etc.
[0205] Based on the amount of polymer (A) used being 100 parts by weight, the amount of epoxy compound used is generally less than 40 parts by weight, and preferably 0.1 parts by weight to 30 parts by weight.
[0206] The aforementioned silane compounds with functional groups may include, but are not limited to, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, N-ethoxycarbonyl-3-aminopropyltriethoxysilane, and N-triethoxysilyl Propyltriethylenetriamine, N-trimethoxysilylpropyltriethylenetriamine, 10-trimethoxysilyl-1,4,7-triacryldecane, 10-triethoxysilyl-1,4,7-triacryldecane, 9-trimethoxysilyl-3,6-diacrylnonyl acetate, 9-triethoxysilyl-3,6-diacrylnonyl acetate, N-benzyl-3-aminopropyltrimethoxysilane, N-benzyl-3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, N-bis(ethylene oxide)-3-aminopropyltrimethoxysilane, N-bis(ethylene oxide)-3-aminopropyltriethoxysilane, etc.
[0207] Based on the amount of polymer (A) used being 100 parts by weight, the amount of silane compound used is generally less than 10 parts by weight, and preferably 0.5 parts by weight to 10 parts by weight.
[0208] Based on the amount of polymer (A) used being 100 parts by weight, the amount of additive (D) used can be from 0.5 parts by weight to 50 parts by weight, and more preferably from 1 part by weight to 45 parts by weight.
[0209] Preparation method of liquid crystal alignment agent
[0210] The preparation method of the liquid crystal alignment agent of the present invention is not particularly limited, and a general mixing method can be used. For example, a first polymer (A1) and a selective second polymer (A2) are first mixed to form a polymer (A). Then, the polymer (A) is mixed with a solvent (B), an amide compound (C), and an additive (D) at a temperature of 0°C to 200°C, and stirred continuously with a stirring device until dissolved. Preferably, the polymer (A), the amide compound (C), and the additive (D) are added to the solvent (B) at a temperature of 20°C to 60°C.
[0211] Method for forming liquid crystal alignment film
[0212] The present invention also provides a liquid crystal alignment film formed from the aforementioned liquid crystal alignment agent. In one embodiment, the liquid crystal alignment agent may be coated on a substrate and subjected to pre-baking, post-baking, and photoalignment treatment to form the liquid crystal alignment film.
[0213] The substrate coated with the liquid crystal alignment agent of the present invention is selected from transparent materials. These transparent materials include, but are not limited to, alkali-free glass, soda-lime glass, hard glass (Pellegrino glass), quartz glass, polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, etc., used in liquid crystal display devices. Preferably, an ITO electrode for liquid crystal driving is already formed on the substrate to simplify the process. Furthermore, for reflective liquid crystal displays with only a single-sided substrate, the aforementioned substrate can be made of an opaque material such as a silicon wafer. In this case, the electrode can be formed using a light-reflecting material such as aluminum. The coating method for the liquid crystal alignment agent of the present invention can be, for example, spin coating, printing, inkjet printing, etc.
[0214] The liquid crystal alignment agent of this invention can be applied at any temperature and for any time for drying and baking. Generally, to fully remove the contained organic solvents, drying at 50°C to 120°C for 1 to 10 minutes is required. Afterward, baking at 150°C to 300°C for 5 to 120 minutes is performed. There is no particular limitation on the thickness of the coating after baking, but an excessively thin coating will degrade the reliability of the liquid crystal display; therefore, a coating thickness of 5 nm to 300 nm is preferable, with 10 nm to 200 nm being even more ideal.
[0215] Although the liquid crystal alignment agent of the present invention can be subjected to conventional rubbing alignment treatment, it is even more effective when using photoalignment treatment.
[0216] Specific examples of the photoalignment treatment method include: irradiating the surface of the aforementioned coating film with radiation polarized in a specific direction, and then heating it at a temperature of 150°C to 250°C, as appropriate, to impart liquid crystal alignment energy to the coating film. Ultraviolet or visible light with wavelengths of 100nm to 800nm can be used as the radiation, with ultraviolet light with wavelengths of 100nm to 400nm being preferred, and ultraviolet light with wavelengths of 200nm to 400nm being even more preferred. Furthermore, to improve liquid crystal alignment, the coating substrate can be irradiated with radiation while being heated at 150°C to 250°C. The preferred irradiation dose of the aforementioned radiation is 1 mJ / cm². 2 Up to 10,000 mJ / cm 2 And with 100mJ / cm 2 Up to 5,000 mJ / cm 2 For even better results, the liquid crystal alignment film prepared in the above manner can stably align liquid crystal molecules in a certain direction.
[0217] The liquid crystal alignment agent of the present invention is subjected to pre-baking treatment, post-baking treatment and photoalignment treatment to form a liquid crystal alignment film, wherein the pretilt angle of the liquid crystal alignment film is 0° to 3°.
[0218] Manufacturing method of liquid crystal display components
[0219] The present invention also provides a liquid crystal display component comprising the aforementioned liquid crystal alignment film.
[0220] The manufacturing method of liquid crystal display components is well known to those skilled in the art, therefore, it will only be briefly described below.
[0221] See Figure 1 A preferred embodiment of the liquid crystal display component 100 of the present invention includes a first unit 110, a second unit 120 and a liquid crystal unit 130, wherein the second unit 120 is spaced apart from the first unit 110 and the liquid crystal unit 130 is disposed between the first unit 110 and the second unit 120.
[0222] The first unit 110 includes a first substrate 112, a first conductive film 114 and a first liquid crystal alignment film 116, wherein the first conductive film 114 is formed on the surface of the first substrate 112 in a pectin pattern, and the first liquid crystal alignment film 116 is formed on the surface of the first conductive film 114.
[0223] The second unit 120 includes a second substrate 122 and a second liquid crystal alignment film 126, wherein the second liquid crystal alignment film 126 is formed on the surface of the second substrate 122.
[0224] The first substrate 112 and the second substrate 122 are selected from transparent materials, including but not limited to alkali-free glass, soda-lime glass, hard glass (Pyles glass), quartz glass, polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, etc., used in liquid crystal display devices. The first conductive film 114 is made of a transparent conductive film selected from tin oxide (SnO2), indium oxide-tin oxide (In2O3-SnO2), etc.; or a metal conductive film such as chromium.
[0225] The first liquid crystal alignment film 116 and the second liquid crystal alignment film 126 are the liquid crystal alignment films mentioned above. Their function is to enable the liquid crystal cell 130 to form a pretilt angle, and the liquid crystal cell 130 can be driven by the parallel electric field generated by the first conductive film 114.
[0226] The liquid crystal used in the liquid crystal unit 130 can be used alone or in combination. The liquid crystals include, but are not limited to, diaminobenzene-based liquid crystals, pyridazine-based liquid crystals, Schiff base-based liquid crystals, azo-based liquid crystals, biphenyl-based liquid crystals, phenylcyclohexane-based liquid crystals, biphenyl-based liquid crystals, ester-based liquid crystals, terphenyl-based liquid crystals, biphenylcyclohexane-based liquid crystals, pyrimidine-based liquid crystals, dioxane-based liquid crystals, bicyclooctane-based liquid crystals, and cubane-based liquid crystals. Furthermore, depending on requirements, additional substances such as cholesterol chloride, cholesterol nonanoate, and cholesterol carbonate can be added. Cholesterol-type liquid crystals such as carbonate, or chiral agents with trade names such as "C-15" or "CB-15" (manufactured by Merck), or ferroelectric liquid crystals such as p-decoxybenzyl methylene-p-amino-2-methylbutyl cinnamate.
[0227] The liquid crystal alignment agent of this invention is suitable for liquid crystal display components made from various types of nematic liquid crystals, such as TN, STN, TFT, VA, and IPS liquid crystal display components. Furthermore, depending on the selected liquid crystal, it can also be used in liquid crystal display components with strong or negative strong conductivity. Among the aforementioned liquid crystal display components, it is particularly suitable for IPS-type liquid crystal display components.
[0228] The present invention will be described in detail by way of the following examples, but it should not be construed as the present invention being limited to the contents disclosed in these examples.
[0229] Synthetic polymer (A1)
[0230] Synthesis example A1-1
[0231] A nitrogen inlet, stirrer, condenser, and thermometer were installed on a 500 mL four-necked conical flask, and nitrogen gas was introduced. Then, 0.045 mol (90 mol%) of p-diaminebenzene (b1-2-1), 0.005 mol (10 mol%) of b1-2-6 diamine compound, and 80 g of N-methyl-2-pyrrolidone (hereinafter referred to as NMP) were added, and the mixture was stirred at room temperature until dissolved. Next, 0.005 mol (10 mol%) of a1-1-1 tetracarboxylic acid dianhydride compound, 0.045 mol (90 mol%) of 2,3,5-tricarboxycyclopentylacetic dianhydride (a1-2-1), and 20 g of NMP were added, and the reaction was carried out at room temperature for 2 hours. After the reaction was complete, the reaction solution was poured into 1500 mL of water to precipitate the polymer. The obtained polymer was filtered, and the washing and filtration steps were repeated three times with methanol. The product was then placed in a vacuum oven and dried at 60°C to obtain polymer (A1-1), the formulation of which is shown in Table 1.
[0232] Synthetic Examples A1-1 to A1-12
[0233] Synthetic Examples A1-1 to A1-12 use the same preparation method as the polymer (A1-1) of Synthetic Example A1-1, except that the types and amounts of raw materials in the polymer are changed in Synthetic Examples A1-1 to A1-12. Their formulations are shown in Table 1 and will not be described again here.
[0234]
[0235] In Table 1:
[0236]
[0237] Synthetic polymer (A2)
[0238] Synthesis Examples A2-1 to A2-6
[0239] Synthetic Examples A2-1 to A2-6 use the same preparation method as the polymer (A1-1) of Synthetic Example A1-1. The difference is that the types and amounts of raw materials in the polymer are changed in Synthetic Examples A2-1 to A2-6. Their formulations are shown in Table 2 and will not be described again here.
[0240] Table 2:
[0241]
[0242] In Table 2:
[0243]
[0244] Synthetic amide compounds (C)
[0245] Synthetic Example C1
[0246] 0.031 mol of the polyol compound of formula (I-2-1), 0.125 mol of acetic acid, and 0.57 g of 4-dimethylaminopyridine were placed in a 1-liter four-necked flask. 125 mL of dichloromethane was added, and 7 g of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide was added while stirring. After the addition was complete, the mixture was stirred at room temperature for 8 hours.
[0247] After the reaction was completed, water was added for two extractions. The organic layer was collected and anhydrous magnesium sulfate was added to remove the water before filtration. The filtrate was then dried under vacuum to remove the solvent, and the remaining solid product, amide compound (C-1), was collected.
[0248] Synthesis example C2
[0249] By replacing acetic acid with propionic acid in synthesis example C1, and keeping all other raw materials and process conditions the same as in synthesis example C1, the amide compound (C-2) can be obtained.
[0250] Synthesis example C3
[0251] By replacing acetic acid with butyric acid in synthesis example C1, and keeping all other raw materials and process conditions the same as in synthesis example C1, the amide compound (C-3) can be obtained.
[0252] Synthetic Example C4
[0253] By replacing acetic acid with n-valeric acid in synthesis example C1, and keeping all other raw materials and process conditions the same as in synthesis example C1, the amide compound (C-4) can be obtained.
[0254] Synthesis Example C5
[0255] By replacing acetic acid with hexanoic acid in synthesis example C1, and keeping all other raw materials and process conditions the same as in synthesis example C1, the amide compound (C-5) can be obtained.
[0256] Synthetic Example C6
[0257] By replacing acetic acid with n-heptanoic acid in synthesis example C1, and keeping all other raw materials and process conditions the same as in synthesis example C1, the amide compound (C-6) can be obtained.
[0258] Synthesis example C7
[0259] By replacing the polyol compound of formula (I-2-1) in synthesis example C1 with the polyol compound of formula (I-2-3) and replacing acetic acid with propionic acid, while keeping all other raw materials and process conditions the same as in synthesis example C1, the amide compound (C-7) can be obtained.
[0260] Synthesis example C8
[0261] By replacing the polyol compound of formula (I-2-1) in synthesis example C1 with the polyol compound of formula (I-2-2) and replacing acetic acid with propionic acid, while keeping all other raw materials and process conditions the same as in synthesis example C1, the amide compound (C-8) can be obtained.
[0262] Synthesis example C9
[0263] By replacing acetic acid with isobutyric acid in synthesis example C1, and keeping all other raw materials and process conditions the same as in synthesis example C1, the amide compound (C-9) can be obtained.
[0264] Synthetic Example C10
[0265] By replacing acetic acid with 3-methylbutyric acid in synthesis example C1, and keeping all other raw materials and process conditions the same as in synthesis example C1, the amide compound (C-10) can be obtained.
[0266] Example 1
[0267] Preparation of liquid crystal alignment agent
[0268] Weigh 10 parts by weight of polymer (A1-1) of synthesis example A1-1, 90 parts by weight of polymer (A2-1) of synthesis example A2-1, and 1800 parts by weight of NMP, and stir and mix them at room temperature to obtain the liquid crystal alignment agent of Example 1.
[0269] Preparation of liquid crystal alignment film and liquid crystal display component
[0270] The aforementioned liquid crystal alignment agent was spin-coated onto a glass substrate, on which pixel electrodes were formed. These pixel electrodes were IPS driving electrodes having a pair of ITO electrodes (electrode width: 10 μm, electrode spacing: 10 μm, electrode height: 50 nm). The pair of ITO electrodes each had a serrated shape, and the serrated portions were arranged in a separated yet interlocking manner. The glass substrate coated with the liquid crystal alignment agent was then dried on a heating plate at 80°C for 5 minutes, followed by baking in a hot air circulating oven at 250°C for 60 minutes to form a coating with a thickness of 100 nm.
[0271] A substrate with a liquid crystal alignment film is prepared by irradiating the coated surface with ultraviolet light at a wavelength of 254 nm through a polarizing plate. Next, a coating is formed on a counter substrate, which is a glass substrate without electrodes but with columnar spacers of 4 μm in height, and an alignment treatment is applied.
[0272] The two substrates are grouped together. A sealant is printed on one substrate, and the other substrate is bonded to the other substrate with the liquid crystal alignment film facing each other and the alignment direction at 0°. The sealant is then cured to obtain an empty cell. This empty cell is injected with liquid crystal MLC-2041 (manufactured by Merck) using a depressurized injection method, and the injection port is sealed, which is the liquid crystal display component of Example 1.
[0273] The liquid crystal display component of Example 1 was evaluated using the evaluation method described below, and the results are shown in Table 3-1.
[0274] Examples 2 to 18 and Comparative Examples 1 to 2
[0275] Examples 2 to 18 and Comparative Examples 1 to 2 used the same preparation method as the liquid crystal alignment agent in Example 1. The difference was that the types and amounts of raw materials in the liquid crystal alignment agent were changed in Examples 2 to 18 and Comparative Examples 1 to 2. The formulations and evaluation results are shown in Tables 3-1, 3-2 and 4, respectively, and will not be described again here.
[0276] Table 3-1:
[0277]
[0278] Table 3-2:
[0279]
[0280] Table 4:
[0281]
[0282] Tables 3-1, 3-2, and 4:
[0283]
[0284] flicker test
[0285] The liquid crystal display components of Examples 1 to 18 and Comparative Examples 1 to 2 were placed between two polarizing plates arranged in a perpendicularly intersecting manner along their polarization axes. The LED backlight was illuminated without any applied voltage, and the arrangement angle of the liquid crystal display components was adjusted to minimize the brightness of the transmitted light. Next, an AC voltage with a frequency of 30 Hz was applied to the liquid crystal display components, and the VT curve (voltage-transmittance curve) was simultaneously measured. The AC voltage with a relative transmittance of 23% was calculated and used as the driving voltage.
[0286] The flicker measurement method involves turning off the lit LED backlight at a temperature of 23°C for the liquid crystal display (LCD) module, placing it in a darkened environment for 72 hours, then turning it back on. Simultaneously with the backlight activation, an AC voltage of 30Hz with a relative transmittance of 23% is applied to drive the LCD module for 60 minutes, and the flicker amplitude is tracked. The flicker amplitude is measured using a data acquisition / recording switching device 34970A (manufactured by Agilent Technologies) connected to a photodiode and an IV converter, reading the brightness value passing through two polarizing plates and the LCD module in between. The flicker is calculated using the following formula (V), where a lower flicker indicates a better quality LCD module made with the liquid crystal alignment agent.
[0287]
[0288] In formula (V), z is the brightness value read when the device 34970A described above is driven by an AC voltage of 30 Hz at a frequency of 23% relative transmittance.
[0289] ◎: Flicker rate <3%
[0290] ○: 4% > flickering intensity ≥ 3%
[0291] △: 5% > flicker ≥ 4%
[0292] X: Flicker level ≥ 5%.
[0293] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the invention. Modifications and variations made to the above embodiments by those skilled in the art do not depart from the spirit of the present invention. The scope of the present invention should be as set forth in the claims.
Claims
1. A liquid crystal alignment agent, comprising: Polymer (A), comprising a first polymer (A1) and a second polymer (A2); Solvent (B); and An amide compound (C) having the structure shown in formula (I-1): Formula (I-1) In formula (I-1), A represents an aliphatic hydrocarbon group with 1 to 20 carbon atoms, an alicyclic group with 3 to 30 carbon atoms, an aromatic hydrocarbon group with 6 to 30 carbon atoms, or a heterocyclic group with 6 to 30 carbon atoms. L1, L2, L3, and L4 each independently represent alkyl groups with 1 to 10 carbon atoms; Ra, Rb, Rc, and Rd each independently represent an alkyl group having 1 to 6 carbon atoms; and in: The first polymer (A1) is prepared by reacting a first mixture comprising a tetracarboxylic dianhydride component (a1) and a diamine component (b1), wherein the tetracarboxylic dianhydride component (a1) comprises at least one tetracarboxylic dianhydride compound (a1-1) as shown in formula (II): Equation (II) In formula (II), R1, R2, R3 and R4 each independently represent a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group containing a fluorine atom and having 1 to 6 carbon atoms, or a phenyl group. R1, R2, R3 and R4 may be the same or different, and at least one of R1, R2, R3 and R4 is not a hydrogen atom. The diamine component (b1) comprises at least one diamine compound (b1-1) selected from diamine compounds having the structure shown in formula [A-1], diamine compounds having the structure shown in formula [A-2], and diamine compounds having the structure shown in formula [A-3]: Formula [A-1] Formula [A-2] Formula [A-3] In formulas [A-1] to [A-3], R5 and R6 each independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a protecting group, and at least one of them is a protecting group; R7, R8, and R9 each independently represent a hydrogen atom, a monovalent hydrocarbon group having 1 to 20 carbon atoms, or a monovalent hydrocarbon group having 1 to 20 carbon atoms with a substituent; D represents a protecting group; The second polymer (A2) is prepared by reacting a second mixture comprising a tetracarboxylic dianhydride component (a2) and a diamine component (b2), wherein the tetracarboxylic dianhydride component (a2) is another tetracarboxylic dianhydride compound (a1-2), and the diamine component (b2) is another diamine compound (b1-2); Based on the total amount of polymer (A) used being 100 parts by weight, the amount of the first polymer (A1) used being 5 to 85 parts by weight, and the amount of the second polymer (A2) used being 15 to 95 parts by weight. Based on the amount of polymer (A) used being 100 parts by weight, the amount of solvent (B) used being 800 to 3000 parts by weight, and the amount of amide compound (C) used being 1 to 20 parts by weight.
2. The liquid crystal alignment agent according to claim 1, wherein the total amount of the tetracarboxylic dianhydride component (a1) used is 100 moles, and the amount of the tetracarboxylic dianhydride compound (a1-1) shown in formula (II) used is from 10 moles to 80 moles.
3. The liquid crystal alignment agent according to claim 1, wherein the total amount of the diamine component (b1) used is 100 moles, and the amount of the diamine compound (b1-1) used is from 0.1 moles to 30 moles.
4. A liquid crystal alignment film formed from a liquid crystal alignment agent as described in any one of claims 1 to 3.
5. The liquid crystal alignment film as described in claim 4, wherein the liquid crystal alignment agent is formed by pre-baking, post-baking and photoalignment treatment.
6. A liquid crystal display assembly comprising the liquid crystal alignment film as described in claim 4 or 5.
Citation Information
Patent Citations
Method for orienting liquid crystal
JP1997297313A
Liquid crystal aligning agent, liquid crystal alignment film and liquid crystal display element
CN108027537A
Liquid crystal aligning agent, liquid crystal alignment layer, method for producing liquid crystal alignment layer, and liquid crystal display element
JP2011237755A