Single-phase bimodal propylene / ethylene / 1-butene random terpolymer compositions with improved optical and sealing properties

By preparing a single-phase bimodal propylene/ethylene/1-butene random terpolymer composition, the shortcomings of existing PP terpolymer-based cast films in terms of low sealing initiation temperature, high clarity, and low hexane extractability are overcome, achieving a combination of good thermal adhesion and processing performance.

CN118019771BActive Publication Date: 2026-11-20BOREALIS AG
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202280063082.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-09-23
Filing Date
2022-09-22
Publication Date
2026-11-20
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

Existing PP terpolymer-based cast films have shortcomings in terms of low sealing initiation temperature, high clarity, and low hexane extractability, making it difficult to simultaneously meet the requirements of good thermal adhesion and processing performance.

Method used

A single-phase bimodal propylene/ethylene/1-butene random terpolymer composition was prepared by using a single-active-center catalyst in two polymerization reactors. By controlling the content of ethylene and 1-butene and the melt flow rate, defects in the 2,1-region were reduced, resulting in a composition with specific properties.

Benefits of technology

It achieves film properties with low sealing initiation temperature of 100 to 115°C, high clarity of 90 to 100%, and low hexane extractability of 0.00 to 0.70%, and has good thermal adhesion and processing properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004746117460000111
    Figure BDA0004746117460000111
  • Figure BDA0004746117460000131
    Figure BDA0004746117460000131
Patent Text Reader

Abstract

A single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) comprising: a) 40 to 90 wt% of a first random terpolymer fraction (PP1) having a C2 content in the range of 0.3 to 3.0 mol% and a C4 content in the range of 1.0 to 5.0 mol%; and b) 10 to 60 wt% of a second random terpolymer fraction (PP2) having a C2 content in the range of 3.0 to 7.0 mol% and a C4 content in the range of 2.0 to 6.0 mol%, having: i) a C2 content in the range of 1.0 to 4.0 mol%; ii) a C4 content in the range of 1.5 to 4.5 mol%; iii) an MFR2 in the range of 3.0 to 10 g / 10 min; and iv) a content of 2,1 regiodefects in the range of 0.1 to 1.5 mol%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP), articles comprising said composition, particularly films, and a method for producing said composition. Background Technology

[0002] Optimization of cast films based on polypropylene (PP) copolymers is a multifaceted problem. Numerous attempts have been made to optimize materials suitable for the films. WO 2002 / 057342 A1 describes biaxially oriented PP (BOPP) films made from copolymers derived from a Ziegler-Natta catalyst comprising at least 0.8 wt%, particularly 0.8 to 1.5 wt%, of ethylene. Although PP terpolymers are speculatively mentioned, such materials are not disclosed in this example. Cast films made from PP copolymers exhibit undesirable high haze. WO 2009 / 019169 A1 describes a method for providing a Ziegler-Natta catalyst-derived PP terpolymer suitable for blown films, comprising at least 8 wt% of a comonomer, wherein the comonomer units are derived from ethylene and C4 to C8 α-olefins using a 1,3-diether internal donor catalyst. According to WO 2009 / 019169A1, an optimal balance of performance should be observed when an ethylene content of less than 2.5 wt% is combined with a 1-butene-1 content of more than 10 wt%, wherein optionally, when the ethylene content is more than 2.5 wt%, the 1-butene content should be less than 10 wt%. Compositions with an ethylene content of 1.2 wt% and 11.3 wt% 1-butene, i.e., a C4 / C2 (wt / wt) ratio of 9.4, result in a SIT as low as 107.4 °C and a haze of 0.2% (1 mm sample). However, these films have unacceptably high levels of hexane (C6) extractability, at 2.8 wt% or higher. US 6,388,040 relates to BOPP films, i.e., completely different types of films made from compositions with different melting temperatures.

[0003] EP 3192817 A1 discloses a method for providing terpolymers comprising units derived from 1-butene using crosslinked metallocene compounds. The terpolymers produced by this method have a high amount of ethylene and a high amount of 1-butene.

[0004] EP 1358252 A1 discloses C3 / C2 / C4 terpolymers with a melting temperature of 155°C or higher.

[0005] WO 2013 / 174778 discloses propylene-based terpolymers of C2, C3, and C4 monomer units produced by Ziegler-Natta catalysts. According to WO 2013 / 174778, the SIT (Self-Induced Tolerance) is reported to be below 110°C, such as 106°C. However, the XCS (Extractable Solids) is relatively high at 25°C, ranging from 5 to 15% by weight, and the disclosed films have unacceptably high levels of hexane (C6) extractable (FDA), at 1.8 or higher.

[0006] Therefore, PP terpolymer-based cast films are still required, which have low sealing onset temperatures (e.g., not greater than 115°C), high clarity (e.g., at least 90%), and particularly low hexane extractability (FDA) (e.g., less than 1.00% by weight). Simultaneously, the film should possess good thermal tack properties.

[0007] This invention addresses these aspects based on the discovery that by utilizing bimodal C3 / C2 / C4 terpolymers with a certain content of 2,1-region defects, a favorable combination of low hexane extractability, high clarity, good processability, and good sealing performance can be provided. Summary of the Invention

[0008] This invention is based on the discovery that a single-phase bimodal propylene / ethylene / 1-butene terpolymer with specific properties including the final composition and the content of each component with defined melt flow rate and comonomer content has improved optical and sealing properties.

[0009] This invention relates to a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP), comprising:

[0010] a) A first random terpolymer portion (PP1) comprising 40 to 90% by weight relative to the total weight of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition, having a permeability in the range of 0.3 to 3.0 mol%. 13 Ethylene content (C2) determined by C-NMR spectroscopy and in the range of 1.0 to 5.0 mol%. 13 The content of 1-butene (C4) determined by C-NMR spectroscopy; and

[0011] b) A second random terpolymer portion (PP2) comprising 10 to 60% by weight of the total weight of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition, having a permeability in the range of 3.0 to 7.0 mol%. 13 Ethylene content (C2) determined by C-NMR spectroscopy and in the range of 2.0 to 6.0 mol%. 13 The 1-butene content (C4) was determined by C-NMR spectroscopy.

[0012] The first random terpolymer portion (PP1) and the second random terpolymer portion (PP2) together constitute at least 95% by weight of the total weight of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP), wherein the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has each of the following properties:

[0013] i) Through the range of 1.0 to 4.0 mol%. 13 Ethylene content (C2) determined by C-NMR spectroscopy;

[0014] ii) Passing within the range of 1.5 to 4.5 mol%. 13 The 1-butene content (C4) was determined by C-NMR spectroscopy;

[0015] iii) Melt flow rate (MFR2) measured at 230°C under a load of 2.16 kg in the range of 3.0 to 10 g / 10 min, according to ISO 1133;

[0016] iv) Quantitative analysis within the range of 0.1 to 1.5 mol%. 13 The content of 2,1-region defects was determined by C-NMR spectroscopy.

[0017] In another embodiment, this application relates to a method for producing the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) of the present invention, comprising the steps of:

[0018] a) Polymerizing propylene, ethylene and 1-butene comonomer units in a first polymerization reactor in the presence of a single active site catalyst to produce a first polymerization mixture comprising the first random terpolymer portion (PP1) and the single active site catalyst, wherein the first polymerization reactor is preferably a slurry reactor, more preferably a loop reactor;

[0019] b) Transferring the first polymerization mixture to a second polymerization reactor, preferably a gas-phase reactor;

[0020] c) In the second polymerization reactor, in the presence of the single-active-site catalyst, polymerize propylene, ethylene and 1-butene comonomer units to produce a second polymerization mixture comprising the first random terpolymer portion (PP1), the second random terpolymer portion (PP2) and the single-active-site catalyst;

[0021] d) Remove the second polymerization mixture from the second polymerization reactor;

[0022] e) Optionally, with the addition of additives, the second polymerization mixture is compounded to form the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

[0023] In a final aspect, the present invention relates to an article, more preferably a film, comprising at least 75% by weight, more preferably at least 90% by weight, and most preferably at least 95% by weight of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) of the present invention. Detailed Implementation

[0024] definition

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. While any methods and materials similar to or equivalent to those described herein may be used in practice to test the invention, preferred materials and methods are described herein. In describing and claiming protection for this invention, the following terms will be used according to their definitions.

[0026] Unless otherwise expressly stated, the terms “a”, “an”, etc., refer to one or more.

[0027] In the following text, unless otherwise stated, quantities are given in weight % (wt%).

[0028] Propylene homopolymers are polymers that are essentially composed of propylene monomer units. Due to impurities, particularly those from industrial polymerization processes, propylene homopolymers may include up to 0.1 mol% comonomer units, preferably up to 0.05 mol% comonomer units, and most preferably up to 0.01 mol% comonomer units.

[0029] Propylene random copolymers are copolymers of propylene monomer units and comonomer units, preferably selected from ethylene and C4-C8 α-olefins, wherein the comonomer units are randomly distributed along the polymer chain. Propylene random copolymers may include comonomer units derived from one or more comonomers with different carbon atomic weights.

[0030] Propylene random terpolymers are random copolymers as described above, which include propylene and two different comonomer units, typically propylene, ethylene and C4-C8 α-olefins.

[0031] Pseudo-terpolymers made from mixtures of two copolymers (e.g., mixtures of propylene / ethylene copolymers and propylene / 1-butene copolymers) are not considered "terpolymers" according to the invention. Pseudo-terpolymers can be identified by coupling TREF-IR, coupling TREF-NMR, or similar methods.

[0032] A typical characteristic of single-phase propylene homopolymers and single-phase propylene random copolymers (including single-phase propylene random terpolymers) is that they have only one glass transition temperature.

[0033] A bimodal polymer is a polymer with a bimodal distribution exhibiting one or more properties. Bimodal random propylene terpolymers can typically be bimodal in terms of comonomer content or in terms of molecular weight (as seen by the melt flow rates of the first and final compositions).

[0034] Detailed description

[0035] Single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP)

[0036] The monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) comprises a first random terpolymer portion (PP1) of 40 to 90% by weight relative to the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition and a second random terpolymer portion (PP2) of 10 to 60% by weight relative to the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition.

[0037] More preferably, the bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) comprises a first random terpolymer portion (PP1) of 50 to 85% by weight relative to the total weight of the monophase bimodal propylene / ethylene / 1-butene random terpolymer composition and a second random terpolymer portion (PP2) of 15 to 50% by weight relative to the total weight of the monophase bimodal propylene / ethylene / 1-butene random terpolymer composition.

[0038] Particularly preferred is that the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) comprises 60 to 80% by weight of a first random terpolymer portion (PP1) relative to the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition, and 20 to 40% by weight of a second random terpolymer portion (PP2) relative to the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition.

[0039] The first random terpolymer portion (PP1) and the second random terpolymer portion (PP2) together constitute at least 95% by weight of the total weight of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

[0040] In addition to the first random terpolymer portion (PP1) and the second random terpolymer portion (PP2), the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) may include other additives known in the art; however, this remaining portion should not exceed 5.0% by weight, such as 3.0% by weight, in the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP). For example, the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) may additionally include small amounts of additives (A) selected from the group consisting of antioxidants, stabilizers, fillers, colorants, nucleating agents, and antistatic agents. Generally, these can be incorporated during the compounding of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

[0041] In the case of a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) containing an α-nucleating agent, it is preferable that it does not contain a β-nucleating agent. The α-nucleating agent is preferably selected from the group consisting of:

[0042] (i) Salts of monocarboxylic and polycarboxylic acids, such as sodium benzoate or aluminum tert-butylbenzoate, and

[0043] (ii) Dibenzyl sorbitol (e.g., 1,3:2,4-dibenzyl sorbitol) and C1-C8-alkyl-substituted dibenzyl sorbitol derivatives, such as methyl dibenzyl sorbitol, ethyl dibenzyl sorbitol, or dimethyl dibenzyl sorbitol (e.g., 1,3:2,4-di(methylbenzyl)sorbitol), or substituted nonitol derivatives, such as 1,2,3,-trideoxy-4,6:5,7-bis-O-[(4-propylphenyl)methylene]-nonitol, and

[0044] (iii) Salts of phosphate diesters, such as sodium 2,2'-methylenebis(4,6'-di-tert-butylphenyl)phosphate or aluminum bis[2,2'-methylene-bis(4,6-di-tert-butylphenyl)phosphate] (or simply aluminum 2,2'-methylene-bis(4,6-di-tert-butylphenyl)phosphate), and

[0045] (iv) Vinylcycloalkane polymers and vinylalkane polymers (described in detail below), and

[0046] (v) Its mixture.

[0047] These additives are generally commercially available and described, for example, in Hans Zweifel's "Plastic Additives Handbook", pp. 871-873, 5th edition, 2001.

[0048] It should be understood that the amount of additive (A) given relative to the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) includes any carrier polymer used to introduce the additive into the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP), i.e., a masterbatch carrier polymer. An example of such a carrier polymer is a polypropylene homopolymer in powder form.

[0049] In one particular embodiment, the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) comprises a first random terpolymer portion (PP1), a second random terpolymer portion (PP2), and an optional additive (A).

[0050] First random terpolymer portion (PP1)

[0051] The first random terpolymer portion (PP1) is a terpolymer of propylene, ethylene, and 1-butene.

[0052] The first random terpolymer portion (PP1) has a content in the range of 0.3 to 3.0 mol%, more preferably in the range of 0.5 to 2.5 mol%, and most preferably in the range of 1.0 to 2.0 mol%. 13 Ethylene content (C2) determined by C-NMR spectroscopy.

[0053] The first random terpolymer portion (PP1) has a content in the range of 1.0 to 5.0 mol%, more preferably in the range of 1.5 to 4.0 mol%, and most preferably in the range of 2.0 to 3.0 mol%. 13 The 1-butene content (C4) was determined by C-NMR spectroscopy.

[0054] The first random terpolymer portion (PP1) preferably has a melt flow rate (MFR2) measured according to ISO 1133 at 230°C and under a load of 2.16 kg, which is in the range of 1.0 to 10 g / 10 min, more preferably in the range of 3.0 to 8.0 g / 10 min, and most preferably in the range of 5.0 to 7.0 g / 10 min.

[0055] Second random terpolymer portion (PP2)

[0056] The second random terpolymer portion (PP2) is a terpolymer of propylene, ethylene, and 1-butene.

[0057] The second random terpolymer portion (PP2) has a content in the range of 3.0 to 7.0 mol%, more preferably in the range of 3.5 to 6.0 mol%, and most preferably in the range of 4.0 to 5.5 mol%. 13 Ethylene content (C2) determined by C-NMR spectroscopy.

[0058] The second random terpolymer portion (PP2) has a content in the range of 2.0 to 6.0 mol%, more preferably in the range of 2.5 to 5.5 mol%, and most preferably in the range of 3.0 to 5.0 mol%. 13 The 1-butene content (C4) was determined by C-NMR spectroscopy.

[0059] The second random terpolymer portion (PP2) preferably has a melt flow rate (MFR2) measured according to ISO 1133 at 230°C and under a load of 2.16 kg, which is in the range of 1.0 to 20.0 g / 10 min, more preferably in the range of 3.0 to 17.0 g / 10 min, and most preferably in the range of 5.0 to 14.0 g / 10 min.

[0060] Properties of single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP)

[0061] The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has a melt flow rate (MFR2) measured according to ISO 1133 at 230°C and under a 2.16 kg load, in the range of 3.0 to 10.0 g / 10 min, more preferably in the range of 4.0 to 9.0 g / 10 min, and most preferably in the range of 5.0 to 8.0 g / 10 min.

[0062] As previously mentioned, the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) can be bimodal in terms of molecular weight (as shown by the melt flow rate value). Therefore, it is preferred that the melt flow rate (MFR2) of both the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) and the melt flow rate (MFR2) of the first random terpolymer portion (PP1) be measured according to ISO 1133 at 230°C under a load of 2.16 kg and expressed in g / 10 min, and that the ratio ([MFR(PP)] / [MFR(PP1)]) is preferably in the range of 0.50 to 1.50, more preferably in the range of 0.80 to 1.30, and most preferably in the range of 1.00 to 1.20.

[0063] The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has a permeability in the range of 1.0 to 4.0 mol%, more preferably in the range of 1.5 to 3.7 mol%, and most preferably in the range of 2.0 to 3.5 mol%.13 Ethylene content (C2) determined by C-NMR spectroscopy.

[0064] The monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) is bimodal in terms of comonomer content, i.e., bimodal in terms of ethylene content, 1-butene content, or both. Therefore, the ethylene content C2 (PP1) of the first random terpolymer portion differs from the ethylene content C2 (PP2) of the second random terpolymer portion, and / or the 1-butene content C4 (PP1) of the first random terpolymer portion differs from the 1-butene content C4 (PP2) of the second random terpolymer portion.

[0065] As mentioned earlier, the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) can be bimodal in terms of ethylene content. Therefore, it is preferable that the ethylene content of both the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) and the ethylene content of the first random terpolymer fraction (PP1) are quantitatively determined. 13 The ratio ([C2(PP)] / [C2(PP1)]) determined by C-NMR spectroscopy and expressed as mol%, is in the range of 1.00 to 4.00, more preferably in the range of 1.10 to 3.00, and most preferably in the range of 1.20 to 2.50.

[0066] The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has a permeability in the range of 2.0 to 6.0 mol%, more preferably 2.5 to 5.5 mol%, and most preferably 3.0 to 5.0 mol%. 13 The 1-butene content (C4) was determined by C-NMR spectroscopy.

[0067] As mentioned earlier, the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) can be bimodal in terms of 1-butene content. Therefore, it is preferable that the 1-butene content of both the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) and the 1-butene content of the first random terpolymer fraction (PP1) are quantitatively determined. 13 The ratio ([C2(PP)] / [C2(PP1)]) determined by C-NMR spectroscopy and expressed as mol% is in the range of 1.00 to 2.00, more preferably in the range of 1.05 to 1.50, and most preferably in the range of 1.10 to 1.30.

[0068] The presence of defects in the 2,1-region of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) indicates that the random propylene copolymer (R-PP) has been polymerized in the presence of a single active site catalyst (SSC).

[0069] Therefore, it is also preferred that the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has been polymerized in the presence of a single active center catalyst (SSC), or more preferably a metallocene catalyst.

[0070] The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) also has the following properties: in the range of 0.10 to 1.50 mol%, more preferably in the range of 0.15 to 1.00 mol%, and most preferably in the range of 0.20 to 0.80 mol%, by quantitative analysis. 13 The content of defects in the 2,1-region was determined by C-NMR spectroscopy. The content of defects in the 2,1-region may depend on the amount of comonomer; higher amounts of comonomer are generally associated with lower contents of defects in the 2,1-region.

[0071] The 2,1-region defect content may also depend on the polymerization temperature; higher temperatures are generally associated with lower 2,1-region defect content.

[0072] The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) preferably has a xylene cold soluble content (XCS) determined according to ISO 16152 in the range of 1.00 to 4.00% by weight, more preferably in the range of 1.5 to 3.5% by weight, and most preferably in the range of 1.80 to 3.00% by weight.

[0073] The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) preferably has a content in the range of 0.00 to 1.00 wt%, more preferably in the range of 0.00 to 0.80 wt%, and most preferably in the range of 0.00 to 0.70 wt%, according to FDA method (C6). FDA The hexane-soluble portion of ).

[0074] Further preferred single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to FDA method (C6) FDA The ratio between the hexane-soluble fraction and the xylene cold soluble content (XCS) determined according to ISO 16152 ([C6) FDA The value of [XCS] is in the range of 0.10 to 0.70, more preferably in the range of 0.15 to 0.50, and most preferably in the range of 0.20 to 0.40.

[0075] Since the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) is not a multiphase system including an elastomer rubber layer, the bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) preferably does not have a glass transition temperature below -30°C, more preferably does not have a glass transition temperature below -25°C, and most preferably does not have a glass transition temperature below -20°C.

[0076] The preferred single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has a melting temperature determined by DSC analysis in the range of 120 to 140°C, more preferably in the range of 125 to 135°C, and most preferably in the range of 127 to 133°C.

[0077] Preferably, the melting temperature has a relevant enthalpy of melting determined by DSC analysis in the range of 50 to 80 J / g, more preferably in the range of 60 to 77 J / g, and most preferably in the range of 65 to 75 J / g.

[0078] It is also preferred that the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has a crystallization temperature determined by DSC analysis in the range of 88 to 97°C, more preferably in the range of 89 to 96°C, and most preferably in the range of 90 to 95°C.

[0079] The preferred single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has at least one of a variety of properties typically used to characterize films, as measured on a 50 μm cast film produced from the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

[0080] Therefore, the preferred single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has a seal initiation temperature (SIT) measured on a 50 μm cast film sample in the range of 100 to 115 °C, more preferably in the range of 101 to 110 °C, and most preferably in the range of 102 to 108 °C.

[0081] The preferred single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has a thermal tack strength measured on a 50 μm cast film sample according to ASTM F1921-12-Method B in the range of 2.0 to 5.0 N, more preferably in the range of 2.5 to 4.5 N, and most preferably in the range of 3.0 to 4.0 N.

[0082] It is also preferred that the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has a longitudinal (MD) tensile modulus measured on a 50 μm cast film sample according to ISO 527-3 in the range of 300 to 700 MPa, more preferably in the range of 400 to 650 MPa, and most preferably in the range of 450 to 600 MPa.

[0083] Further preferred is a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) having a haze value measured on a 50 μm cast film sample according to ASTM D1003 in the range of 0.0 to 3.0%, more preferably in the range of 0.0 to 2.5%, and most preferably in the range of 0.0 to 2.0%.

[0084] The preferred single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) has a clarity value measured on a 50 μm cast film sample according to ASTM D1003 in the range of 90 to 100%, more preferably in the range of 92 to 100%, and most preferably in the range of 94 to 100%.

[0085] method

[0086] The present invention further relates to a method for producing a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to the present invention.

[0087] The method includes the following steps:

[0088] a) Polymerizing propylene, ethylene and 1-butene comonomer units in the presence of a single active site catalyst in a first polymerization reactor (R1) to produce a first polymerization mixture comprising the first random terpolymer portion (PP1) and the single active site catalyst, wherein the first polymerization reactor (R1) is preferably a slurry reactor (SR), more preferably a loop reactor (LR).

[0089] b) Transfer the first polymerization mixture to a second polymerization reactor (R2), preferably a gas-phase reactor (GPR);

[0090] c) In the second polymerization reactor (R2), in the presence of the single-active-site catalyst, polymerize propylene, ethylene and 1-butene comonomer units to produce a second polymerization mixture comprising the first random terpolymer portion (PP1), the second random terpolymer portion (PP2) and the single-active-site catalyst;

[0091] d) Remove the second polymerization mixture from the second polymerization reactor (R2); and

[0092] e) Optionally, with the addition of additives, the second polymerization mixture is compounded to form the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

[0093] Preferably, the operating temperature in the first polymerization reactor (R1) is in the range of 62 to 85°C, more preferably in the range of 65 to 82°C, and even more preferably in the range of 67 to 80°C.

[0094] As an alternative to or supplement to the previous step, it is preferable that the operating temperature in the second polymerization reactor (R2) is in the range of 75 to 95°C, more preferably in the range of 78 to 92°C.

[0095] Typically, the pressure in the first polymerization reactor (R1), preferably the loop reactor (LR), is in the range of 20 to 80 bar, preferably 30 to 70 bar, for example 35 to 65 bar, while the pressure in the second polymerization reactor (R2), i.e. the gas phase reactor (GPR), is in the range of 5 to 50 bar, preferably 15 to 40 bar.

[0096] Preferably, hydrogen is added to each polymerization reactor to control the molecular weight, i.e., the melt flow rate MFR2.

[0097] In addition to the (primary) polymerization of propylene random terpolymers in two polymerization reactors (R1 and R2), the preparation of propylene random terpolymers may also include prepolymerization in a prepolymerization reactor (PR) upstream of the first polymerization reactor (R1).

[0098] Polypropylene (Pre-PP) is produced in a prepolymerization reactor (PR). Prepolymerization is carried out in the presence of a single active site catalyst (SSC). According to this embodiment, the single active site catalyst is introduced into the prepolymerization step. However, this does not preclude the option of adding additional co-catalysts at later stages, such as in the polymerization process, for example, in the first reactor (R1). In one embodiment, if prepolymerization is applied, all components of the single active site catalyst are added only to the prepolymerization reactor (PR).

[0099] The prepolymerization reaction is typically carried out at temperatures of 0 to 60°C, preferably 15 to 50°C, and more preferably 20 to 45°C.

[0100] The pressure in the prepolymerization reactor is not critical, but it must be high enough to keep the reaction mixture in the liquid phase. Therefore, the pressure can be from 20 to 100 bar, for example, from 30 to 70 bar.

[0101] In a preferred embodiment, prepolymerization is carried out by bulk slurry polymerization in liquid propylene, i.e., the liquid phase mainly comprises propylene, optionally containing dissolved inert components. Furthermore, according to the invention, as described above, ethylene is used as feedstock during the prepolymerization process.

[0102] Other components may also be added during the prepolymerization stage. Therefore, as is known in the art, hydrogen can be added to the prepolymerization stage to control the molecular weight of polypropylene (Pre-PP). Furthermore, antistatic additives can be used to prevent particles from adhering to each other or to the reactor walls.

[0103] Precise control of prepolymerization conditions and reaction parameters is within the scope of the art.

[0104] Due to the aforementioned defined process conditions in prepolymerization, it is preferable to obtain a mixture (MI) of single active site catalyst (SSC) and polypropylene (Pre-PP) produced in the prepolymerization reactor (PR). Preferably, the single active site catalyst (SSC) is (finely) dispersed in the polypropylene (Pre-PP). In other words, the single active site catalyst (SSC) particles introduced into the prepolymerization reactor (PR) are broken into smaller fragments, which are uniformly distributed within the grown polypropylene (Pre-PP). The size of the introduced single active site catalyst (SSC) particles and the resulting fragments are not important to this invention and are within the knowledge of those skilled in the art.

[0105] As described above, if prepolymerization is used, after the prepolymerization, the mixture (MI) of the single active site catalyst (SSC) and polypropylene (Pre-PP) produced in the prepolymerization reactor (PR) is transferred to the first reactor (R1). Typically, the total amount of polypropylene (Pre-PP) in the final bimodal propylene terpolymer (PP) is quite low and typically does not exceed 5.0% by weight, more preferably not exceed 4.0% by weight, and even more preferably in the range of 0.5 to 4.0% by weight, for example in the range of 1.0 to 3.0% by weight.

[0106] Without using prepolymerization, propylene and other components, such as single active center catalyst (SSC), are directly introduced into the first polymerization reactor (R1).

[0107] In one embodiment, the present invention relates to a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) as described above, which can be obtained by the methods described herein, more preferably by the methods described herein. All preferred embodiments and alternative positions given above and below for the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) are applicable with necessary modifications.

[0108] catalyst system

[0109] The single-active-site catalyst according to the present invention can be any supported metallocene catalyst suitable for producing isotactic polypropylene.

[0110] Preferred single-active-site catalysts (SSCs) include metallocene complexes, cocatalyst systems including boron-containing cocatalysts and / or aluminoxane cocatalysts, and silica supports.

[0111] In particular, preferred single-active-center catalysts (SSCs) include

[0112] (i) Metallocene complexes having the general formula (I)

[0113]

[0114] Each X is independently a σ-donor ligand.

[0115] L is a divalent bridge selected from -R'2C-, -R'2C-CR'2-, -R'2Si-, -R'2Si-SiR'2-, and -R'2Ge-, wherein each R' is independently a hydrogen atom or optionally contains one or more heteroatoms or fluorine atoms from groups 14 to 16 of the periodic table. 20 - A hydrocarbon group, or any two R' groups together, can form a ring.

[0116] Each R 1 Independently identical or may be different, and is hydrogen, straight-chain or branched C1-C6-alkyl group, C 7-20 -Aryl group, C 7-20 - alkylaryl group or C 6-20 -Aryl group or OY group, where Y is C 1-10 - hydrocarbon group, and optionally two adjacent R 1 The groups can be part of a ring that includes the phenyl carbon to which they are bonded.

[0117] Each R 2 Independently identical or may be different, and is CH2-R 8 Group, wherein R 8 Is it H or straight chain or branched chain C? 1-6 -alkyl group, C 3-8 -cycloalkyl group, C 6-10 -Aryl group,

[0118] R 3 It is a straight-chain or branched C1-C6-alkyl group, C 7-20 -Aryl group, C 7-20 -Alkyl group or C6-C 20 -Aryl group, R 4 It is C(R) 9 )3 groups, of which R 9 It is a straight-chain or branched C1-C6-alkyl group.

[0119] R 5 It is hydrogen or optionally contains one or more heteroatoms from groups 14 to 16 of the periodic table, and is an aliphatic C1-C group. 20 - Hydrocarbon group;

[0120] R 6 It is hydrogen or optionally contains one or more heteroatoms from groups 14 to 16 of the periodic table, and is an aliphatic C1-C group.20 - hydrocarbon group; or

[0121] R 5 and R 6 They can together form a 5-membered saturated carbon ring, which is optionally bound by n groups R. 10 Replacement, where n is 0 to 4;

[0122] Each R 10 Same or different, and can be C1-C 20 - A hydrocarbon group, or optionally a C1-C group containing one or more heteroatoms belonging to groups 14 to 16 of the periodic table. 20 - Hydrocarbon group;

[0123] R 7 It is an H or a straight-chain or branched C1-C6-alkyl group or optionally surrounded by 1 to 3 R groups. 11 Substituted aryl or heteroaryl groups having 6 to 20 carbon atoms, each R 11 Independently identical or may be different and is hydrogen, straight-chain or branched C1-C6-alkyl group, C 7-20 -Aryl group, C 7-20 - alkylaryl group or C 6-20 -Aryl group or OY group, where Y is C 1-10 -Hydrocarbon group,

[0124] (ii) Catalyst systems including boron-containing cocatalysts and / or aluminum oxane cocatalysts, and

[0125] (iii) Silica carrier.

[0126] The term "σ-donor ligand" is well known to those skilled in the art, referring to a group that bonds to a metal via a σ bond. Therefore, the anionic ligand "X" can be independently a halogen or selected from the group consisting of R', OR', SiR'3, OSiR'3, OSO2CF3, OCOR', SR', NR'2, or PR'2, wherein R' is independently hydrogen, straight-chain or branched, cyclic or acyclic, C1 to C2. 20 Alkyl, C2 to C 20 alkenyl, C2 to C 20 alkynyl group, C3 to C 12 cycloalkyl, C6 to C 20 Aryl, C7 to C 20 Arane, C7 to C 20 Alkyl, C8 to C 20 Arylalkenyl, wherein the R' group may optionally contain one or more heteroatoms belonging to groups 14 to 16. In a preferred embodiment, the anionic ligand "X" is identical and is a halogen, such as Cl, or methyl or benzyl.

[0127] Preferred monovalent anionic ligands are halogens, especially chlorine (Cl).

[0128] Preferred metallocene catalyst complexes include: racemic-dimethylsilylbis[2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylindene-1-yl]zirconium dichloride, racemic-trans-dimethylsilyl[2-methyl-4-(4'-tert-butylphenyl)-indene-1-yl][2-methyl-4-(4'-tert-butylphenyl)-5-methoxy-6-tert-butylindene-1-yl]zirconium dichloride, racemic-trans-dimethylsilylbis[ ... Zirconium dichloride, racemic-trans-dimethylsilyl[2-methyl-4-(3',5'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-indarsen-1-yl][2-methyl-4-(3',5'-dimethyl-phenyl)-5-methoxy-6-tert-butylindarsen-1-yl]di Zirconium chloride, racemic-trans-dimethylsilyl[2-methyl-4,8-bis-(4'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-indarsen-1-yl][2-methyl-4-(3',5'-dimethyl-phenyl)-5-methoxy-6-tert-butylindene-1-yl]zirconium dichloride, racemic-trans-dimethylsilyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s- Zirconium dichloride [2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylindene-1-yl], racemic-trans-dimethylsilyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indene-1-yl], Zirconium dichloride

[0129] Particularly preferred is racemic-trans-dimethylsilyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indarsen-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylindene-1-yl]zirconium dichloride.

[0130] The ligands required to form the complex and thus the catalyst of this invention can be synthesized by any process, and a skilled organic chemist will be able to design various synthetic schemes for producing the necessary ligand materials. For example, WO 2007 / 116034 discloses the necessary chemical processes. Synthetic schemes can also generally be found in WO 2002 / 02576, WO 2011 / 135004, WO 2012 / 084961, WO 2012 / 001052, WO 2011 / 076780, WO 2015 / 158790 and WO 2018 / 122134. Particular reference is made to WO 2019 / 179959, which describes the most preferred catalyst of this invention.

[0131] co-catalyst

[0132] In order to form an active catalytic substance, a co-catalyst well known in the art is usually required.

[0133] According to the present invention, a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst is used in combination with a metallocene catalyst complex as defined above.

[0134] Aluminoxane co-catalysts can be one of formula (II):

[0135]

[0136] Where n is typically between 6 and 20 and R has the following meanings.

[0137] Aluminoxanes are formed through the partial hydrolysis of organoaluminum compounds, such as those of the formula AlR3, AIR2Y, and Al2R3Y3, wherein R can be, for example, C1-C 10 Alkyl, preferably C1-C5 alkyl, or C3-C 10 cycloalkyl, C7-C 12 Aryl or alkylaryl and / or phenyl or naphthyl, wherein Y can be hydrogen, halogen, preferably chlorine or bromine, or C1-C 10 Alkoxy, preferably methoxy or ethoxy. The resulting oxyaluminoxane is usually not a pure compound, but a mixture of oligomers of formula (II).

[0138] The preferred aluminoxane is methylaluminoxane (MAO). Since the aluminoxane used as a cocatalyst according to the present invention is not a pure compound due to its preparation method, the molar concentration of the aluminoxane solution hereinafter is based on its aluminum content.

[0139] According to the present invention, a boron-containing cocatalyst can be used instead of an aluminum oxane cocatalyst, or an aluminum oxane cocatalyst can be used in combination with a boron-containing cocatalyst.

[0140] Those skilled in the art will understand that, when using a boron-based cocatalyst, the complex is typically pre-alkylated by reacting it with an alkylaluminum compound (e.g., TIBA). This procedure is well-known and any suitable alkylaluminum can be used, such as Al(C1-C6 alkyl)3. Preferred alkylaluminum compounds are triethylaluminum, triisobutylaluminum, triisohexylaluminum, tri-n-octylaluminum, and triisooctylaluminum.

[0141] Alternatively, when using a borate cocatalyst, the metallocene catalyst complex is in its alkylated form, i.e., a dimethyl or dibenzyl metallocene catalyst complex can be used.

[0142] Boron-based cocatalysts of interest include those of formula (III).

[0143] BY3(III),

[0144] Wherein Y may be the same or different, and is a hydrogen atom, an alkyl group having 1 to about 20 carbon atoms, an aryl group having 6 to about 15 carbon atoms, an alkylaryl group, an aralkyl group, a haloalkyl group, or a haloaryl group (each alkyl group having 1 to 10 carbon atoms and each aryl group having 6 to 20 carbon atoms), or fluorine, chlorine, bromine, or iodine. Preferred options are trifluoroborane, triphenylborane, tri(4-fluorophenyl)borane, tri(3,5-difluorophenyl)borane, tri(4-fluoromethylphenyl)borane, tri(2,4,6-trifluorophenyl)borane, tri(pentafluorophenyl)borane, tri(tolyl)borane, tri(3,5-dimethyl-phenyl)borane, tri(3,5-difluorophenyl)borane, and / or tri(3,4,5-trifluorophenyl)borane.

[0145] Tris(pentafluorophenyl)borane is particularly preferred.

[0146] However, borates, i.e., compounds containing borate 3+ ions, are preferred. Such ionic cocatalysts preferably contain noncoordinate anions, such as tetra(pentafluorophenyl)borate and tetraphenylborate. Suitable counterions are protonated amines or aniline derivatives, such as methylammonium, phenylammonium, dimethylammonium, diethylammonium, N-methylphenylammonium, diphenylammonium, N,N-dimethylphenylammonium, trimethylammonium, triethylammonium, tri-n-butylammonium, methyldiphenylammonium, pyridinium, p-bromo-N,N-dimethylphenylammonium, or p-nitro-N,N-dimethylphenylammonium. Surprisingly, certain boron cocatalysts have been found to be particularly preferred. Therefore, the preferred borates used in this invention include triphenylmethyl ions. Therefore, N,N-dimethylammonium tetrapentafluorophenylboronic acid and Ph3CB(PhF5)4 and their analogues are particularly preferred.

[0147] The preferred cocatalyst is aluminum oxane, more preferably methyl aluminum oxane, a combination of aluminum oxane and alkyl aluminum, boron or borate cocatalyst, and a combination of aluminum oxane and boron-based cocatalyst.

[0148] The catalyst system of the present invention is used in a supported form. The particulate support material used is silica or a mixed oxide such as silica-alumina, particularly silica. Silica support is preferred. Those skilled in the art understand the procedures required for supporting metallocene catalysts.

[0149] In a preferred embodiment, the catalyst system corresponds to ICS3 of WO 2020 / 239598 A1.

[0150] Products

[0151] In the final embodiment, the present invention relates to an article comprising at least 75% by weight, more preferably at least 90% by weight, and most preferably at least 95% by weight, a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

[0152] In addition to the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP), other polymer components may be present in the product; however, it is preferred that the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) is the only polymer component in the product.

[0153] In a particularly preferred embodiment, the article comprises a monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

[0154] The product according to the present invention is preferably a film, and more preferably a cast film.

[0155] The preferred film, more preferably the cast film, has a thickness in the range of 5 to 100 μm, more preferably in the range of 10 to 80 μm, and most preferably in the range of 20 to 70 μm.

[0156] The film according to the invention, more preferably the cast film, preferably has a sealing initiation temperature (SIT) in the range of 100 to 115°C, more preferably in the range of 101 to 110°C, and most preferably in the range of 102 to 108°C.

[0157] The film according to the invention, more preferably the cast film, preferably has a thermal tack strength measured according to ASTM F1921-12-Method B in the range of 2.0 to 5.0 N, more preferably in the range of 2.5 to 4.5 N, and most preferably in the range of 3.0 to 4.0 N.

[0158] The film according to the invention, more preferably the cast film, preferably has a longitudinal (MD) tensile modulus measured according to ISO 527-3 in the range of 300 to 700 MPa, more preferably in the range of 400 to 650 MPa, and most preferably in the range of 450 to 600 MPa.

[0159] The film according to the invention, more preferably the cast film, preferably has a haze value measured according to ASTM D1003 in the range of 0.0 to 3.0%, more preferably in the range of 0.0 to 2.5%, and most preferably in the range of 0.0 to 2.0%.

[0160] The film according to the invention, more preferably the cast film, preferably has a clarity value measured according to ASTM D1003 in the range of 90 to 100%, more preferably in the range of 92 to 100%, and most preferably in the range of 94% to 100%.

[0161] The film, more preferably the cast film, can be a single-layer film. Alternatively, the film, more preferably the cast film, can exist as a single layer in a multilayer film.

[0162] When the film exists as a single layer in a multilayer film, it can be prepared by any means known in the art. Preferably, the multilayer film is prepared by co-extrusion of a cast film.

[0163] Example

[0164] A. Measurement Method

[0165] Unless otherwise defined, the following definitions and determination methods apply to the above general description of the invention, including the claims, and the following embodiments.

[0166] Quantification of microstructure using NMR spectroscopy

[0167] Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the comonomer content of the polymer.

[0168] Quantitative 13 C{ 1 HNMR spectroscopy is used for 1 H and 13 Recordings were taken in the molten state using a Bruker Avance III 500 NMR spectrometer operating at 500.13 and 125.76 MHz, respectively. Nitrogen gas was used for all pneumatic devices, and the system was operated at 180 °C. 13All spectra were recorded using a C-optimized 7mm magic angle rotation (MAS) probe. Approximately 200 mg of material was loaded into a 7mm outer diameter zirconia MAS rotor and rotated at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification. Standard single-pulse excitation was employed with a short 3s cycle delay using NOE and RS-HEPT decoupling schemes. A total of 1024 (1k) transient signals were acquired for each spectrum.

[0169] Quantitative 13 C{ 1 The ¹H NMR spectra were processed, integrated, and the quantitative properties were determined from the integration. All chemical shifts were internally referenced at 21.85 ppm for the methyl isotactic pentatonic group (mmmm).

[0170] The characteristic signal {brandolini01} corresponding to the incorporation of 1-butene was observed and the content of comonomers was quantified.

[0171] The amount of isolated 1-butene incorporated into the PBP sequence was quantified by integrating the αB2 site at 43.6 ppm and taking into account the number of reporter sites for each comonomer:

[0172] B = I αB2 / 2

[0173] The amount of 1-butene sequentially incorporated into the PBBP sequence was quantified by integrating the ααB2B2 site at 40.5 ppm and taking into account the number of reporter sites for each comonomer:

[0174] BB = 2 * I ααB2B2

[0175] In the presence of BB, the value of B must be corrected based on the effect of the αB2 site generated by BB:

[0176] B = (I αB2 / 2)–BB / 2

[0177] The total 1-butene content is calculated based on the sum of isolated and continuously incorporated 1-butene:

[0178] B 总 =B+BB

[0179] The characteristic signal {brandolini01} corresponding to the incorporation of ethylene was observed, and the content of comonomers was quantified.

[0180] The amount of isolated ethylene incorporated into the PEP sequence was quantified by integrating the Sββ site at 24.3 ppm and taking into account the number of reporter sites for each comonomer:

[0181] E = I Sββ

[0182] If a characteristic signal corresponding to the continuous incorporation of ethylene in the PEE sequence is observed, quantification is performed using the Sβδ site at 27.0 ppm:

[0183] EE = I Sβδ

[0184] The characteristic signal {resconi00} corresponding to the regional defect was observed. The presence of an isolated 2,1-erythro-type regional defect is indicated by the presence of two methyl sites at 17.7 and 17.2 ppm and a methylene site at 42.4 ppm, and confirmed by other characteristic sites. Two unequal Sαβ signals at 34.8 ppm and 34.4 ppm, respectively, and a Tγγ at 33.7 ppm indicate the presence of a 2,1-regional defect near the ethylene unit.

[0185] Using the integral of the methylene site at 42.4 ppm (I e9 ) to quantify isolated 2,1-Erythian region defects (P 21e孤立 ) quantity:

[0186] P 21e孤立 =I e9

[0187] If present, use the methine site at 33.7 ppm (I Tγγ The amount of defects (P) in the 2,1-region adjacent to ethylene E21 Quantification:

[0188] P E21 =I Tγγ

[0189] The total ethylene content is then calculated based on the sum of isolated, continuously incorporated, and adjacent 2,1-region defects:

[0190] E 总 =E + EE + P E21

[0191] The amount of propylene was quantified based on the Sαα methylene site at 46.7 ppm, which includes all additional propylene units not covered by Sαα, such as the factor 3*P. 21e孤立 This explains the three missing propylene units in the isolated 2,1-erythroide region defect:

[0192] P总 =I Sαα +3*P 21e孤立 +B+0.5*BB+E+0.5*EE+2*P E21

[0193] Then, the total mole fraction of 1-butene and ethylene in the polymer is calculated as follows:

[0194] fB = B 总 / (E 总 +P 总 +B 总 )

[0195] fE=E 总 / (E 总 +P 总 +B 总 )

[0196] The molar percentage of comonomer incorporated is calculated from the mole fraction:

[0197] B[moles%] = 100 * fB

[0198] E[mol%] = 100 * fE

[0199] The weight percentage of comonomer incorporated is calculated as a mole fraction:

[0200] B[weight%] = 100*(fB*56.11) / ((fE*28.05)+(fB*56.11)+((1-(fE+fB))*42.08))

[0201] E[weight%] = 100 * (fE * 28.05) / ((fE * 28.05) + (fB * 56.11) + ((1 - (fE + fB)) * 42.08))

[0202] The molar percentage of isolated 2,1-erythroide region defects relative to all propylene was quantified:

[0203] [21e] mole% = 100*P 21e孤立 / P 总

[0204] The molar percentage of defects in the 2,1-region adjacent to ethylene was quantified relative to all propylene:

[0205] [E21] mole% = 100 * P E21 / P 总

[0206] The total number of defects in 2,1- is quantified as follows:

[0207]

[21] mole% = [21e] + [E21]

[0208] No characteristic signal {resconi00} was observed corresponding to other types of regional defects (2,1-Soviet type, 3,1-insertion type).

[0209] References (as mentioned above):

[0210] klimke06 Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2006; 207:382.

[0211] parkinson07 Parkinson, M., Klimke, K., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2007; 208:2128.

[0212] pollard04 Pollard,M.,Klimke,K.,Graf,R.,Spiess,HW,Wilhelm,M.,Sperber,O.,Piel,C.,Kaminsky,W.,Macromolecules 2004;37:813.

[0213] filip05 Filip,X.,Tripon,C.,Filip,C.,J.Mag.Resn.2005,176,239.

[0214] griffin07 Griffin,JM,Tripon,C.,Samoson,A.,Filip,C.,and Brown,SP,Mag.Res.in Chem.2007 45,S1,S198.

[0215] castignolles09 Castignolles,P.,Graf,R.,Parkinson,M.,Wilhelm,M.,Gaborieau,M.,Polymer 50(2009)2373.

[0216] resconi00 Resconi,L.,Cavallo,L.,Fait,A.,Piemontesi,F.,Chem.Rev.2000,100,1253.

[0217] brandolini01 AJ Brandolini, DDHills, "NMR spectra of polymers and polymer additives", Marcel Deker Inc., 2000.

[0218] Calculation of comonomer content in the second random terpolymer portion (PP2):

[0219]

[0220] in

[0221] w(PPl) is the weight fraction [in weight %] of the first random terpolymer portion (PP1).

[0222] w(PP2) is the weight fraction of the second random terpolymer portion (PP2) [in weight %].

[0223] C(PP1) is the comonomer content [in mole %] of the first random terpolymer portion (PP1).

[0224] C(PP) is the comonomer content [in mol%] of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

[0225] C(PP2) is the calculated comonomer content [in mol%] of the second random terpolymer portion (R-PP2).

[0226] melt flow rate

[0227] Melt flow rate (MFR) is determined according to ISO 1133 and expressed in g / 10 min. MFR characterizes the flowability of a polymer and therefore its processability. A higher melt flow rate generally indicates a lower polymer viscosity. The MFR2 of polypropylene was determined at 230°C and a load of 2.16 kg.

[0228] Calculation of the melt flow rate MFR2 (230℃) of the second random terpolymer portion (PP2):

[0229]

[0230] in

[0231] w(PPl) is the weight fraction [in weight %] of the first random terpolymer portion (PP1).

[0232] w(PP2) is the weight fraction of the second random terpolymer portion (PP2) [in weight %].

[0233] MFR(PP1) is the melt flow rate MFR2 (230°C) of the first random terpolymer moiety (PP1) [in g / 10min].

[0234] MFR(PP) is the melt flow rate MFR2 (230°C) [in g / 10min] of a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

[0235] MFR(PP2) is the calculated melt flow rate of the second random terpolymer portion (PP2) MFR2 (230°C) [in g / 10 min].

[0236] Xylene-soluble fraction at room temperature (XCS, wt%): The amount of polymer soluble in xylene was determined at 25°C according to ISO 16152; 5th edition; 2005-07-01.

[0237] DSC analysis, melting temperature (T) m ) and heat of fusion (H f ), crystallization temperature (T) c ) and heat of crystallization (H c ): Samples of 5 to 7 mg were measured using a TAInstrument Q200 differential scanning calorimetry (DSC). The DSC was operated according to ISO 11357 / Part 3 / Method C2 in a heating / cooling / heating cycle at a scan rate of 10 °C / min, with a temperature range of -30 to +225 °C. Crystallization temperature (T c ) and heat of crystallization (H c The melting temperature (T) is determined by the cooling step, while the melting temperature (T) is determined by the melting step. m ) and heat of fusion (H f The result was determined by the second heating step.

[0238] The glass transition temperature (Tg) was determined by dynamic mechanical analysis according to ISO 6721-7. Measurements were taken from compression-molded samples (40 × 10 × 1 mm) between -100°C and +150°C. 3 The heating was performed in a torsion mode at a rate of 2°C / min and a frequency of 1Hz.

[0239] The hexane-soluble fraction (C6 FDA) was determined by film analysis according to FDA method (Federal Registration, Title 21, Chapter 1, Part 177, Section 1520, s. Annex B). The film was produced on a Collin 30 laboratory-scale cast film production line with a melt temperature of 250°C, a cooling roller temperature of 40°C, and a film thickness of 100 μm.

[0240] The amount of hexane-soluble polymer was determined from the film sample prepared as described above according to the FDA method (Federal Register, Title 21, Chapter 1, Part 177, Section 1520, s. Annex B). The extraction temperature was 50°C and the extraction time was 2 hours.

[0241] Haze and clarity were measured according to ASTM D1003 on a 50 μm thick cast film produced as shown below.

[0242] The tensile modulus in the longitudinal (MD) and transverse (TD) directions was determined according to ISO 527-3 on 50 μm thick cast films produced on a single-layer cast film production line at a melt temperature of 220 °C and a cooling roll temperature of 20 °C, as shown below. The test was conducted at a crosshead speed of 1 mm / min until the yield strength, and then at a speed of 10 mm / min until the sample broke.

[0243] The hot tack was determined on a J&B hot tack tester on a single-layer cast film production line at a melting temperature of 220°C and a cooling roller temperature of 20°C, based on a modified method of ASTM F1921-12-Method B.

[0244] Sample cutting machine:

[0245] Use a roller cutter or strip cutter to cut the sample to a width of 25 mm (±0.5%).

[0246] Test machine:

[0247] • Sealing strip length: 50mm

[0248] • Sealing strip width: 5mm

[0249] • Sealing strip shape: flat

[0250] • Sealing strip material: Brass-Nickel

[0251] • Sealing strip coating:

[0252] • Roughness of the sealing strip: approximately 1 μm

[0253] Force measurement: Piezoelectric force sensor

[0254] • Temperature measurement: 2 independent heating systems

[0255] Thickness measuring equipment: (accuracy according to ISO 4593:1993)

[0256] • Position indicator (Heidenhain; Model: ND 280)

[0257] • Touch probe (Heidenhain; Model: MT 1281)

[0258] Measuring surface: Polished flat / planar surface

[0259] Diameter of each face: 6.5mm

[0260] Sample / test specimen preparation:

[0261] All test specimens must be prepared in standard atmosphere for conditioning and testing at 23°C (±2°C) and 50% (±10%) relative humidity.

[0262] Minimum conditioning time for test specimens in standard atmosphere before starting the test: >16h.

[0263] Minimum storage time between film sample extrusion and start of testing: >88h.

[0264] Sample preparation:

[0265] Specimen type: Parallel cut stripes obtained across the entire width of the specimen, 25 mm (width) × approximately 320 mm (length).

[0266] Sample orientation: machine orientation

[0267] The sample (film) should be free of dust, fingerprints, wrinkles, creases, shrinkage, or other obvious defects. The edges of the cut sample should be smooth and without nicks.

[0268] Thickness measurement:

[0269] The thickness of the test specimen was measured in the sealed area.

[0270] Heat-sealing process:

[0271] The test should be conducted under the same atmospheric conditions as the conditioning.

[0272] Under defined temperature, contact time, and pressure conditions, the two flat heated sealing jaws ( Pressure is applied to seal the prepared sample strip (5*50mm).

[0273] The sample is folded between sealing jaws using an automated sample folding device. The jaws close, and after a preset sealing time, they open, completing the heat seal. After a selected cooling time, the lower sample clamp moves downwards. During the sample pulling process, a force sensor attached to the upper sample clamp measures the force. The fault mode is then visually determined.

[0274] Standard test conditions:

[0275] • Sealing temperature (ambient temperature - 240℃)

[0276] • Sealing time (thickness <25μm: 0.5s; thickness ≥25μm: 1s)

[0277] • Sealing pressure (0.15 N / mm) 2 )

[0278] • Delay time (0.2s)

[0279] • Fixture separation rate (200 mm / s)

[0280] Note: Parameter values ​​can be freely selected by the user.

[0281] Number of test specimens: at least 3 specimens per temperature.

[0282] If a temperature step measurement shows a significant deviation, ensure it is an outlier and test another sample (the number of samples should always be non-uniform, but the total number of samples tested should not exceed 7) to allow the outlier to be removed from the measurement - other causes of deviation must be considered.

[0283] Temperature step / interval: 5℃↑

[0284] (2℃↑ if there is a sharp increase / decrease between two temperature steps)

[0285] Measurements were started at two temperature steps below 0.2 to 0.3 N.

[0286] Stop measurement when the failure mode is burn-through.

[0287] It also allows for one failure mode with burn-through and two other failure modes - plus an additional temperature step.

[0288] A typical thermoviscosity curve may require 25 to 50 samples for each material.

[0289] result:

[0290] The output of this method is a thermoviscosity curve. The interpretation of the thermoviscosity curve always depends on the relationship between sealing force and sealing temperature.

[0291] Hot tack: The highest force with the failure mode "peel". When using 3 specimens / temperature steps, two "peel" failure modes and any other failure mode (except burn-through failure mode) are also allowed.

[0292] Deviating from ASTM F1921-12 Chapter 9, the test was conducted after a 200 ms cooling time. The measurement termination described in ASTM F1921-12 Chapter 9.8 (testing stops after thermal viscosity is determined) was not considered. The test ended after film thermal failure. Additional failure modes were used in addition to the failure mode assessments described in the standard.

[0293] Sealing start temperature (SIT)

[0294] This method is used to determine the sealing window (sealing temperature range) of a film. The procedure is similar to that of thermal viscous measurement, but unlike thermal viscous measurement, the sealing range applies to the strength of the seal (or closure) after cooling (with a delay time of 30 s).

[0295] Sealing range = (Sealing start temperature to sealing end temperature)

[0296] The determined results provide users with a quantitative and useful indication of the strength of the sealing film and show the temperature range for optimal sealing.

[0297] The temperature interval is set to 5°C by default, but when the curve shows a sharp increase or decrease in force between two temperature steps, the temperature interval can be reduced to 1°C to represent a better curve profile.

[0298] Deviating from ASTM F1921-12, the test parameters—sealing pressure, cooling time, and test speed—were modified. Force / temperature profiling continued until film thermal failure. Additional failure modes were used in addition to those described in the standard for failure mode assessment.

[0299] To characterize the material, the sealing range initiation temperature (SIT), the temperature at maximum force (MAX), and the sealing range end temperature (SET) were also measured.

[0300] Standard conditions:

[0301] Adjustment time: >96h

[0302] Sealing jaw size: 50×5mm

[0303] Sealing jaw shape: flat

[0304] Sealing jaw coating: Niptef

[0305] Sealing temperature: ambient temperature -240℃

[0306] Sealing temperature interval: 5℃

[0307] Sealing time: 1s

[0308] Delay time: 30s

[0309] Sealing pressure: 0.4 N / mm 2 (PE); 0.67 N / mm 2 (PP)

[0310] Grip separation rate: 42 mm / s

[0311] Sealing starting force: 5N

[0312] Sample width: 25mm

[0313] result:

[0314] The output of this method is a sealing curve.

[0315] The lower limit (sealing start temperature - SIT) is the sealing temperature at which a sealing force of ≥5N is obtained.

[0316] B. Example

[0317] The catalyst used in the polymerization processes of all embodiments was the trans-dimethylsilane[2-methyl-4,8-di(3,5-dimethylphenyl)-1,5,6,7-tetrahydro-s-indarsen-1-yl][2-methyl-4-(3,5-dimethylphenyl)-5-methoxy-6-tert-butylindene-1-yl]zirconium dichloride, i.e., MC-2, disclosed in WO 2019 / 179959 A1. The preparation of the supported metallocene catalyst was similar to that of IE2 in WO 2019 / 179959 A1.

[0318] The embodiments of the present invention IE1 to IE4 and comparative examples CE1 and CE2 were polymerized according to the conditions given in Table 1 (Note: The MFR2, C2 and C4 contents given after reactor R2 are the performance of the GPR part and were calculated using appropriate mixing rules based on the values ​​measured after the loop reactor (i.e. PP1) and in the final pellets (i.e. PP).

[0319] CE3 is a propylene / ethylene / 1-butene terpolymer catalyzed by Ziegler-Natta and is commercially available from Borealis AG under the trade name TD310BF.

[0320] Table 1: Polymerization conditions and properties of the propylene / ethylene / 1-butene terpolymer of the present invention and comparison

[0321]

[0322]

[0323] Table 2: Performance of 50 μm cast films made from the propylene / ethylene / 1-butene terpolymer of the present invention and comparison

[0324]

[0325] As shown in Table 2, the clarity of each bimodal embodiment is significantly better than that of the single-peak comparative examples CE1 and CE2. Furthermore, the SIT value is much lower than that of the single-peak compositions.

[0326] Many additional advantages will become apparent to those skilled in the art when the various embodiments are compared.

[0327] At similar comonomer contents, IE1 has significantly better optical performance (haze and sharpness) than CE1 or CE2. In addition, IE1 has lower SIT and similar thermal tack compared to CE2, and lower Tm, lower SIT and improved thermal tack compared to CE1.

[0328] IE2 exhibits similar properties to CE3; however, achieving these properties requires significantly less 1-butene. Furthermore, it demonstrates superior thermal adhesion.

[0329] IE3 and IE4 also have less 1-butene than CE3 and achieve lower Tm, higher thermal tack and similar SIT.

[0330] Furthermore, the embodiments of the present invention exhibit a significantly better ratio of C6 extractable to XCS. CE1 and CE2 require higher 1-butene content to achieve acceptable thermal tack, which results in a higher proportion of XCS content that can also be extracted with hexane. This may lead to problems such as blooming.

[0331] Clearly, compared with the SSC-catalyzed monomodal terpolymers (CE1 and CE2) and the Ziegler-Natta-catalyzed terpolymers (CE3), the SSC-catalyzed bimodal terpolymers of the present invention provide an improved balance between optical and sealing properties.

Claims

1. A single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP), comprising: a) A first random terpolymer portion (PP1) comprising 40 to 90% by weight relative to the total weight of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition, having a permeability in the range of 0.3 to 3.0 mol%. 13 Ethylene content (C2) determined by C-NMR spectroscopy and in the range of 1.0 to 5.0 mol% by [method name missing]. 13 The 1-butene content (C4) determined by C-NMR spectroscopy; and b) A second random terpolymer portion (PP2) comprising 10 to 60% by weight of the total weight of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition, having a permeability in the range of 3.0 to 7.0 mol%. 13 Ethylene content (C2) determined by C-NMR spectroscopy and in the range of 2.0 to 6.0 mol% by [method name missing] 13 The 1-butene content (C4) was determined by C-NMR spectroscopy. The first random terpolymer portion (PP1) and the second random terpolymer portion (PP2) together constitute at least 95% by weight of the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP). The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) described herein has each of the following properties: i) Through the range of 1.0 to 4.0 mol%. 13 Ethylene content (C2) determined by C-NMR spectroscopy; ii) Passing within the range of 1.5 to 4.5 mol%. 13 The 1-butene content (C4) was determined by C-NMR spectroscopy. iii) Melt flow rate MFR2, measured according to ISO 1133 at 230°C under a load of 2.16 kg, in the range of 3.0 to 10 g / 10 min; and iv) Quantitative analysis within the range of 0.1 to 1.5 mol%. 13 The content of 2,1-region defects was determined by C-NMR spectroscopy.

2. The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to claim 1, having a xylene cold soluble content (XCS) in the range of 1.00 to 4.00% by weight, as determined according to ISO 16152.

3. The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to claim 1 or claim 2, having a melting temperature determined by DSC analysis in the range of 120 to 140°C.

4. The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to claim 3, wherein the melting temperature has a relevant enthalpy of melting determined according to DSC analysis in the range of 50 to 80 J / g.

5. The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to claim 1 or 2, wherein... a) The first random terpolymer portion (PP1) has a melt flow rate MFR2 in the range of 1.0 to 10.0 g / 10 min, as determined according to ISO 1133 at 230 °C under a load of 2.16 kg, and b) The second random terpolymer portion (PP2) has a melt flow rate MFR2 in the range of 1.0 to 20.0 g / 10 min, as determined according to ISO 1133 at 230 °C and a load of 2.16 kg. The melt flow rate MFR2 of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) and the melt flow rate MFR2 of the first random terpolymer portion (PP1) are both determined according to ISO 1133 at 230°C under a load of 2.16 kg and expressed in g / 10 min, and their ratio ([MFR(PP)] / [MFR(PP1)]) is in the range of 0.50 to 1.

50.

6. The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to claim 1 or 2, wherein the ethylene content of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) and the ethylene content of the first random terpolymer portion (PP1) are both determined by quantitative analysis. 13 The ratio ([C2(PP)] / [C2(PP1)]) was determined by C-NMR spectroscopy and expressed as mol%, ranging from 1.00 to 4.00, and / or The 1-butene content of the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) and the 1-butene content of the first random terpolymer fraction (PP1) were both determined quantitatively. 13 The values ​​were determined by C-NMR spectroscopy and expressed as mol%, with the ratio ([C2(PP)] / [C2(PP1)]) ranging from 1.00 to 2.

00.

7. The monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to claim 1 or 2, comprising 50 to 85% by weight of a first random terpolymer portion (PP1) relative to the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition, and 15 to 50% by weight of a second random terpolymer portion (PP2) relative to the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition.

8. The monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to claim 7, comprising a first random terpolymer portion (PP1) of 60 to 80% by weight relative to the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition, and a second random terpolymer portion (PP2) of 20 to 40% by weight relative to the total weight of the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition.

9. The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to claim 1 or 2, having a crystallization temperature determined by DSC analysis in the range of 88 to 97°C.

10. The single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to claim 1 or 2, having one or two of the following properties: a) The hexane-soluble fraction (C6) according to FDA methods, ranging from 0.00 to 1.00% by weight. FDA ),as well as b) The hexane-soluble fraction (C6) according to the FDA method, in the range of 0.10 to 0.

70. FDA The ratio between (C6) and the xylene cold soluble content (XCS) determined according to ISO 16152 ([C6) FDA ] / [XCS]).

11. A method for producing a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to any one of claims 1 to 10, comprising the steps of: a) In a first polymerization reactor, propylene, ethylene and 1-butene comonomer units are polymerized in the presence of a single active site catalyst to produce a first polymerization mixture comprising the first random terpolymer portion (PP1) and the single active site catalyst; b) Transfer the first polymerization mixture to the second polymerization reactor; c) In the second polymerization reactor, in the presence of the single-active-site catalyst, polymerize propylene, ethylene and 1-butene comonomer units to produce a second polymerization mixture comprising the first random terpolymer portion (PP1), the second random terpolymer portion (PP2) and the single-active-site catalyst; d) Remove the second polymerization mixture from the second polymerization reactor; and e) Optionally, with the addition of additives, the second polymerization mixture is compounded to form the single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP).

12. The method of claim 11, wherein the first polymerization reactor is a slurry reactor or a loop reactor.

13. The method of claim 11, wherein the second polymerization reactor is a gas-phase reactor.

14. The method according to any one of claims 11 to 13, wherein the single-active-center catalyst comprises: (i) Metallocene complexes having general formula (I) Formula (I) Each X is independently a σ-donor ligand. L is a divalent bridge selected from -R'2C-, -R'2C-CR'2-, -R'2Si-, -R'2Si-SiR'2-, and -R'2Ge-, wherein each R' is independently a hydrogen atom or optionally contains one or more heteroatoms or fluorine atoms from groups 14 to 16 of the periodic table. 20 - A hydrocarbon group, or any two R' groups together, can form a ring. Each R 1 Independently identical or may be different, and is hydrogen, straight-chain or branched C1-C6-alkyl group, C 7-20 -Aryl group, C 7-20 - alkylaryl group or C 6-20 -Aryl group or OY group, where Y is C 1-10 - hydrocarbon group, and optionally two adjacent R 1 The groups can be part of a ring that includes the phenyl carbon to which they are bonded. Each R 2 Independently identical or may be different, and is CH2-R 8 Group, wherein R 8 Is it H or straight chain or branched chain C? 1-6 -alkyl group, C 3-8 -cycloalkyl group, C 6-10 -Aryl group, R 3 It is a straight-chain or branched C1-C6-alkyl group, C 7-20 -Aryl group, C 7-20 -Alkyl group or C6-C 20 -Aryl group, R 4 It is C(R) 9 )3 groups, of which R 9 It is a straight-chain or branched C1-C6-alkyl group. R 5 It is hydrogen or optionally contains one or more heteroatoms from groups 14 to 16 of the periodic table, and is an aliphatic C1-C group. 20 - Hydrocarbon group; R 6 It is hydrogen or optionally contains one or more heteroatoms from groups 14 to 16 of the periodic table, and is an aliphatic C1-C group. 20 - hydrocarbon group; or R 5 and R 6 They can together form a 5-membered saturated carbon ring, which is optionally bound by n groups R. 10 Replacement, where n is 0 to 4; Each R 10 Same or different, and can be C1-C 20 - A hydrocarbon group, or optionally a C1-C group containing one or more heteroatoms belonging to groups 14 to 16 of the periodic table. 20 - Hydrocarbon group; R 7 It is an H or a straight-chain or branched C1-C6-alkyl group or optionally surrounded by 1 to 3 R groups. 11 Substituted aryl or heteroaryl groups having 6 to 20 carbon atoms, Each R 11 Independently identical or may be different and is hydrogen, straight-chain or branched C1-C6-alkyl group, C 7-20 -Aryl group, C 7-20 - alkylaryl group or C 6-20 -Aryl group or OY group, where Y is C 1-10 -Hydrocarbon group, (ii) Catalyst systems including boron-containing cocatalysts and / or aluminoxane cocatalysts, and (iii) Silica carrier.

15. A composition, wherein the composition is a monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to any one of claims 1 to 10, wherein the monophasic bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) can be obtained by the method according to any one of claims 11 to 14.

16. An article comprising at least 75% by weight of a single-phase bimodal propylene / ethylene / 1-butene random terpolymer composition (PP) according to any one of claims 1 to 10 or 15.

17. The article of claim 16, wherein the article is a film.

18. The article of claim 16, wherein the article is a cast film.

19. The article according to any one of claims 16 to 18, having one or two of the following properties: a) Sealing start temperature (SIT) in the range of 100 to 115°C, and b) Thermal tack strength measured according to ASTM F1921-12-Method B in the range of 2.0 to 5.0 N.

20. The article of any one of claims 16 to 18, having a longitudinal (MD) tensile modulus measured according to ISO 527-3 in the range of 300 to 700 MPa.

21. The article according to any one of claims 16 to 18, having one or two of the following properties: a) Haze values ​​measured according to ASTM D1003 in the range of 0.0% to 3.0%, and b) Sharpness values ​​measured according to ASTM D1003 in the range of 90 to 100%.

Citation Information

Patent Citations

  • Bioriented polypropylene films

    EP1358252A2

  • Propylene / ethylene / alpha-olefin terpolymers and processes for the production thereof

    US6388040B1

  • Bridged BIS (indenyl) metallocene compounds

    WO2002002576A1

  • Bioriented polypropylene films

    WO2002057342A2

  • Metallocene compounds

    WO2007116034A1