Alkali-resistant polymer mbr membrane and preparation method thereof
By coating the polymer MBR membrane with an alkali-resistant coating solution, the problem of easy fouling of the polymer MBR membrane in alkaline environment is solved, thereby improving the membrane's alkali resistance and hydrophilicity, extending its service life and improving filtration accuracy.
Patent Information
- Application Number
- CN202410270258.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-11
AI Technical Summary
Existing polymer MBR membranes are prone to irreversible fouling due to alkali cleaning during long-term operation in high ammonia nitrogen water environments. Furthermore, existing modification methods suffer from problems such as migration and loss of modified substances or the formation of defective pores in the membrane after blending.
The method involves coating the surface of a polymer MBR membrane with an alkali-resistant coating solution. Polyvinyl alcohol acetal is used as a macromolecular modifying material. The modified coating solutions of different concentrations are applied to the membrane surface in stages, with the low-concentration coating solution applied before the high-concentration coating solution, to form an alkali-resistant coating and enhance the alkali resistance and adhesion of the membrane.
It improves the membrane's resistance to alkali corrosion, extends its service life, enhances its hydrophilicity and filtration accuracy, and the process is simple and suitable for industrial production.
Smart Images

Figure CN118022551B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of MBR membrane preparation technology, specifically relating to an alkali-resistant polymer MBR membrane and its preparation method. Background Technology
[0002] Polymer-based MBR membranes are prone to irreversible fouling in high-ammonia-nitrogen water environments during long-term operation, necessitating alkaline cleaning. However, membranes made of materials such as PVDF, PVC, and PAN are not alkali-resistant, and the cleaning process can reduce their mechanical properties, thus affecting long-term operational stability and shortening their service life. Therefore, it is necessary to modify polymer-based MBR membranes to improve their alkali resistance for alkaline cleaning.
[0003] In related technologies, patent application CN102382323A discloses a method for improving the alkali corrosion resistance of polyvinylidene fluoride products. It uses a solution blending method to mix perfluoroalkyl amphiphilic molecules with polyvinylidene fluoride and dry them to form a film. During the film formation process, polar perfluoroalkyl amphiphilic molecules migrate to the film surface to form an alkali-resistant layer. However, since the modified substances are all salts and small molecules, they will continuously migrate outward during use, affecting long-term alkali resistance. Patent application CN111484639A discloses a modification method for alkali-resistant PVDF materials. It uses a blending molding method to mix VDF / CTFE diblock copolymer or VDF / TrFE / CTFE triblock copolymer with polyvinylidene fluoride, and forms a film through extrusion, injection molding, casting, calendering and pressing. Although mixing PVDF with alkali-resistant fluorinated copolymer can improve the alkali resistance of PVDF, the compatibility between PVDF and its copolymer is limited, only partially compatible. After blending, large defect pores will be generated in the membrane, affecting the filtration accuracy and anti-fouling performance.
[0004] Therefore, it is necessary to provide an alkali-resistant polymer MBR membrane and its preparation method to solve the problems mentioned in the background art. Summary of the Invention
[0005] This application provides an alkali-resistant polymer MBR membrane and its preparation method. The alkali resistance of the membrane is increased by coating the surface of the polymer MBR membrane with an alkali-resistant coating liquid, which has an interpenetrating network or finger-like pores. The polyvinyl acetal used for modification is a macromolecule, which effectively solves the problem of outward migration and loss of the modified material in CN102382323A. The modification method adopted is surface coating, which effectively solves the problem that the blending method in CN111484639A will cause large defect pores in the membrane.
[0006] To solve the above-mentioned technical problems, the technical solution of this application is as follows:
[0007] A method for preparing an alkali-resistant polymer MBR membrane, characterized by comprising the following steps:
[0008] Step S1: Prepare a polymer MBR base membrane with an interpenetrating network or finger-shaped pores in cross section;
[0009] Step S2: Prepare two modified coating solutions with different concentrations. The modified coating solutions are prepared by dissolving alkali-resistant viscous coating polyvinyl acetal in a second solvent.
[0010] Step S3: The two modified coating solutions are applied to the surface of the polymer MBR base membrane in multiple applications to form an alkali-resistant coating, wherein the lower concentration modified coating solution is applied before the higher concentration modified coating solution.
[0011] Preferably, the polymer MBR base membrane is an unseparated primary base membrane or a wet membrane obtained after the primary base membrane is separated into phases in a room temperature water coagulation bath, and the thickness of the polymer MBR base membrane is 0.240-0.270 mm.
[0012] Preferably, the preparation process of the unseparated primary base film specifically includes the following steps:
[0013] Step S11: According to the mass fraction, 14% of the polymer, 1%-5% of the pore-forming agent and 81%-85% of the first solvent are added to a three-necked flask and mixed. The temperature is raised to 80-90℃ and stirred for 12 hours to obtain the casting solution.
[0014] Step S12: The casting solution is allowed to stand at 70°C to degas, and then poured onto a glass plate heated to 50°C and covered with non-woven fabric to obtain an unseparated nascent base film.
[0015] The wet membrane preparation process, in addition to the unseparated primary base membrane preparation process, also includes the following steps:
[0016] Step S13: Immerse the unseparated nascent base membrane in a pure water coagulation bath at 25°C to further form a membrane. Soak the obtained membrane in clean room temperature water for 48 hours to remove the residual first solvent. Then take out the membrane and wipe the surface of the membrane dry with filter paper to obtain a wet membrane.
[0017] Preferably, the pore-forming agent is selected from at least one of calcium chloride, polyvinylpyrrolidone, and polyethylene glycol; the polymer is selected from one of PVDF, PAN, and PVC; and the first solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, or N-methylpyrrolidone.
[0018] Preferably, the adhesive coating is selected from at least one of polyvinyl alcohol formaldehyde, polyvinyl alcohol acetal, and polyvinyl alcohol butyral; the second solvent is selected from at least one of ethanol, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.
[0019] Preferably, the components of the viscous coatings in the two modified coating solutions are the same.
[0020] Preferably, the two modified coating liquids contain different components of viscous coatings.
[0021] Preferably, in any of the modified coating solutions, the mass fraction of the viscous coating is 5%-10%.
[0022] Preferably, the time interval between applying the two modified coating solutions is not less than 1 minute.
[0023] An alkali-resistant polymer MBR membrane is prepared by the above-described preparation method, wherein the thickness of the alkali-resistant polymer MBR membrane is 0.320 mm.
[0024] The beneficial effects of this application are as follows:
[0025] (1) The selected surface coating material has excellent adhesion, hydrophilicity and alkali resistance. After coating modification, the contact angle becomes smaller, the wetting time is shortened, the hydrophilicity is significantly improved, and the alkali corrosion resistance is increased.
[0026] (2) Two coating solutions with different concentrations are prepared. The low-concentration coating solution is used to penetrate into the base membrane and modify the interior. The high-concentration coating solution is used to modify the surface of the base membrane. The internal and external coating solutions are bonded to each other, which increases the adhesion of the coating and makes it less likely to fall off. This can effectively prevent the membrane from being exposed to alkaline environments during cleaning, and extend the number of cleaning cycles and service life of the membrane.
[0027] (3) The coating obtained by secondary coating can cover the defects and pores on the surface of the base membrane and reduce the pore size, which is beneficial to improving the filtration accuracy.
[0028] (4) The process is simple and suitable for industrial production. Attached Figure Description
[0029] Figure 1 (a) Figure 1 (b) shows the surface microstructure and cross-sectional microstructure of the polymer MBR base membrane, respectively;
[0030] Figure 2 (a) Figure 2 (b) Surface micrographs and cross-sectional micrographs of the alkali-resistant polymer MBR membrane of Example 1, respectively;
[0031] Figures 3(a) and 3(b) show the surface micrograph and cross-sectional micrograph of the alkali-resistant polymer MBR membrane of Example 2, respectively;
[0032] Figure 4 (a) Figure 4 (b) Surface micrographs and cross-sectional micrographs of the alkali-resistant polymer MBR membrane of Example 3, respectively;
[0033] Figure 5 (a) Figure 5 (b) shows the surface micrograph and cross-sectional micrograph of the alkali-resistant polymer MBR membrane of Example 4, respectively;
[0034] Figure 6 A comparison of color changes after various membrane surfaces come into contact with a 1M NaOH solution;
[0035] Figure 7 (a) Figure 7 (b) A comparison diagram showing the contact angles of the polymer MBR base membrane and the alkali-resistant polymer MBR membrane of Example 2. Detailed Implementation
[0036] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0037] Please refer to the following: Figure 1 (a)- Figure 7 (b) This application provides a method for preparing an alkali-resistant polymer MBR membrane, comprising the following steps:
[0038] Step S1: Prepare a polymer MBR base membrane with an interpenetrating network or finger-shaped pores in cross section.
[0039] The polymer MBR base membrane is an unseparated primary base membrane or a wet membrane obtained after the primary base membrane is separated into phases in a room temperature water coagulation bath, and the membrane thickness is 0.240-0.270 mm.
[0040] The preparation process of the unseparated primary base film specifically includes the following steps:
[0041] Step S11: According to the mass fraction, 14% of the polymer, 1%-5% of the pore-forming agent and 81%-85% of the first solvent are added to a three-necked flask and mixed. The temperature is raised to 80-90℃ and stirred for 12 hours to obtain the casting solution.
[0042] Step S12: The casting solution is allowed to stand at 70°C to degas, and then poured onto a glass plate heated to 50°C and covered with nonwoven fabric to obtain an unseparated nascent base film.
[0043] The wet membrane preparation process, in addition to the unseparated primary base membrane preparation process, also includes the following steps:
[0044] Step S13: Immerse the unseparated nascent base membrane in a pure water coagulation bath at 25°C to further form a membrane. Soak the obtained membrane in clean room temperature water for 48 hours to remove the residual first solvent. Then take out the membrane and wipe the surface of the membrane dry with filter paper to obtain a wet membrane.
[0045] The polymer is selected from PVDF (polyvinylidene fluoride), PAN (polyacrylonitrile), and PVC (polyvinyl chloride); the porogen is selected from at least one of calcium chloride, polyvinylpyrrolidone, and polyethylene glycol; the first solvent is selected from at least one of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), and N-methylpyrrolidone (NMP).
[0046] Step S2: Prepare two modified coating solutions with different concentrations. The modified coating solutions are prepared by dissolving alkali-resistant viscous coating polyvinyl acetal in a second solvent.
[0047] The adhesive coating is selected from at least one of polyvinyl formal (PVFM), polyvinyl acetal (PVE), and polyvinyl butyral (PVB); the second solvent is selected from at least one of ethanol, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP).
[0048] Step S3: The two modified coating solutions are applied to the surface of the polymer MBR base membrane in multiple applications to form an alkali-resistant coating, wherein the lower concentration modified coating solution is applied before the higher concentration modified coating solution.
[0049] In any of the modified coating solutions, the mass fraction of the viscous coating is 5%-10%; the time interval between the application of the two modified coating solutions is not less than 1 minute, so that the low-concentration modified coating solution can fully penetrate into the interpenetrating network or finger pores of the polymer MBR base membrane.
[0050] Polyvinyl acetal exhibits excellent adhesion to various materials. Low-concentration modified coating solutions possess strong permeability, allowing them to penetrate effectively into the interpenetrating network or finger-like pores of the polymer MBR base membrane, thus modifying its interior. The good adhesion of polyvinyl acetal allows it to bond well with the interpenetrating network or finger-like pores. Furthermore, during the second coating process, it can form an adhesive bond with high-concentration coating solutions, facilitating the adhesion of the high-concentration coating solution and preventing it from detaching after film formation, thereby extending its service life. High-concentration modified coating solutions have poor permeability but strong adhesion, primarily adhering to the surface of the polymer MBR base membrane. This modifies the surface of the polymer MBR base membrane and reduces its pore size, limiting the escape of low-concentration modified coating solutions from the interior of the polymer MBR base membrane and improving its filtration accuracy.
[0051] Polyvinyl acetal has good alkali resistance. By applying a two-stage modified coating with polyvinyl acetal coating solution, the polymer MBR base membrane has good alkali resistance and can resist short-term low-concentration alkali corrosion during alkali cleaning. At the same time, it endows the polymer MBR base membrane with good hydrophilicity and antifouling properties.
[0052] When the polymer MBR base membrane is selected as an unseparated nascent base membrane, after the modified coating solution is applied, the unseparated nascent base membrane and the alkali-resistant coating are simultaneously introduced into the coagulation bath for phase separation. Since the nascent base membrane has not yet separated before entering the coagulation bath, the alkali-resistant coating will penetrate into the base membrane along with the coating solvent and become entangled with the base polymer, thus maintaining a strong bond with the base membrane.
[0053] When the polymer MBR base membrane is selected as a wet membrane, since the base membrane surface has been phase-separated and formed into pores, and the alkali-resistant coating is a hydrophilic material, the alkali-resistant coating will penetrate into the interior of the membrane pores under the induction of the coating solvent and the water molecules inside the membrane pores, thus allowing the coating to adhere to the base membrane.
[0054] Example 1
[0055] This embodiment provides an alkali-resistant flat-sheet PVDF membrane and its preparation method, specifically including the following steps:
[0056] (1) Preparation of flat PVDF base film
[0057] 14 wt% PVDF, 2 wt% PVP, and 84 wt% DMAc were mixed in a 250 mL three-necked flask. The flask was placed in a 90 °C oil bath and stirred for 12 h to obtain a uniform, pale yellow, transparent casting solution. The casting solution was then transferred to a 70 °C oil bath and allowed to stand for 12 h to degas. The degassed casting solution was poured onto a glass plate heated to 50 °C and covered with nonwoven fabric. The height of the doctor blade on an automatic film scraper was adjusted to 0.400 mm, and the film was scraped at a speed of 3 m / min to obtain an unseparated PVDF nascent base film.
[0058] (2) Preparation of modified coating solution
[0059] 5 wt% PVE, 40 wt% DMAc and 60 wt% ethanol were mixed in a 250 mL three-necked flask. The three-necked flask was placed in a 25 °C water bath and stirred for 12 h to obtain a uniform colorless and transparent casting solution. The casting solution was then allowed to stand for 12 h to remove bubbles, resulting in a 5 wt% PVE coating solution.
[0060] PVB (10wt%), DMAc (45wt%) and ethanol (45wt%) were mixed in a 250mL three-necked flask. The three-necked flask was placed in a 25℃ water bath and stirred for 12h to obtain a uniform, colorless and transparent casting solution. The casting solution was then allowed to stand for 12h to remove bubbles, resulting in a 10wt% PVB coating solution.
[0061] (3) Preparation of alkali-resistant flat-sheet PVDF membrane
[0062] The doctor blade height of the automatic coating machine was adjusted to 0.320 mm, and the coating speed was 3 m / min. A 5 wt% PVE coating solution was poured onto a glass plate coated with an unseparated PVDF nascent base film and coated. The film was left in the air for at least 1 minute to allow the coating solution to penetrate. Then, a 10 wt% PVB coating solution was poured onto the glass plate for a second coating and coating process to obtain the nascent composite film. The nascent composite film was slowly immersed in a room temperature water coagulation bath for further film formation. After removing the film from the coagulation bath, it was soaked in clean room temperature water for 48 hours to remove residual solvent. The film was then transferred to a room temperature glycerol aqueous solution and soaked for 48 hours. Finally, the film was air-dried to obtain an alkali-resistant flat-sheet PVDF film.
[0063] Example 2
[0064] This embodiment provides an alkali-resistant flat-sheet PVDF membrane and its preparation method, specifically including the following steps:
[0065] (1) Preparation of flat PVDF base film
[0066] 14 wt% PVDF, 2 wt% PVP, and 84 wt% DMAc were mixed in a 250 mL three-necked flask. The flask was placed in a 90 °C oil bath and stirred for 12 h to obtain a uniform, pale yellow, transparent casting solution. The casting solution was then transferred to a 70 °C oil bath and allowed to stand for 12 h to degas. The degassed casting solution was poured onto a glass plate heated to 50 °C and covered with nonwoven fabric. The height of the doctor blade on an automatic film scraper was adjusted to 0.400 mm, and the film was scraped at a speed of 3 m / min to obtain an unseparated PVDF nascent base film.
[0067] (2) Preparation of modified coating solution
[0068] 5 wt% PVE, 40 wt% DMAc and 60 wt% ethanol were mixed in a 250 mL three-necked flask. The three-necked flask was placed in a 25 °C water bath and stirred for 12 h to obtain a uniform colorless and transparent casting solution. The casting solution was then allowed to stand for 12 h to remove bubbles, resulting in a 5 wt% PVE coating solution.
[0069] 10 wt% PVE, 45 wt% DMAc and 45 wt% ethanol were mixed in a 250 mL three-necked flask. The three-necked flask was placed in a 25 °C water bath and stirred for 12 h to obtain a uniform colorless and transparent casting solution. The casting solution was then allowed to stand for 12 h to remove bubbles, resulting in a 10 wt% PVE coating solution.
[0070] (3) Preparation of alkali-resistant flat-sheet PVDF membrane
[0071] The doctor blade height of the automatic coating machine was adjusted to 0.320 mm, and the coating speed was 3 m / min. A 5 wt% PVE coating solution was poured onto a glass plate coated with an unseparated PVDF nascent base film, and the film was coated. The plate was left in air for at least 1 minute to allow the coating solution to penetrate. Then, a 10 wt% PVE coating solution was poured onto the glass plate for a second coating and coating process to obtain the nascent composite film. The nascent composite film was slowly immersed in a room temperature water coagulation bath for further film formation. After removing the film from the coagulation bath, it was soaked in clean room temperature water for 48 hours to remove residual solvent. The film was then transferred to a room temperature glycerol aqueous solution and soaked for 48 hours. Finally, the film was air-dried to obtain a PVDF-based alkali-resistant water-treated flat sheet membrane.
[0072] Example 3
[0073] This embodiment provides an alkali-resistant flat-sheet PVDF membrane and its preparation method, specifically including the following steps:
[0074] (1) Preparation of flat PVDF base film
[0075] 14 wt% PVDF, 2 wt% PVP, and 84 wt% DMAc were mixed in a 250 mL three-necked flask. The flask was placed in a 90 °C oil bath and stirred for 12 h to obtain a uniform, pale yellow, transparent casting solution. The casting solution was then transferred to a 70 °C oil bath and allowed to stand for 12 h to degas. The degassed casting solution was poured onto a glass plate heated to 50 °C and covered with nonwoven fabric. The height of the doctor blade of the automatic film scraper was adjusted to 0.400 mm, and the film was scraped at a speed of 3 m / min to obtain an unseparated PVDF primary base film.
[0076] The unseparated PVDF nascent base membrane was immersed in a pure water coagulation bath at 25°C for further membrane formation. The resulting membrane was then soaked in clean room temperature water for 48 hours to remove residual DMAc. The membrane was then removed and the surface moisture was wiped dry with filter paper to obtain a wet flat sheet PVDF base membrane.
[0077] (2) Preparation of modified coating solution
[0078] 5 wt% PVE, 40 wt% DMAc and 60 wt% ethanol were mixed in a 250 mL three-necked flask. The three-necked flask was placed in a 25 °C water bath and stirred for 12 h to obtain a uniform colorless and transparent casting solution. The casting solution was then allowed to stand for 12 h to remove bubbles, resulting in a 5 wt% PVE coating solution.
[0079] 10 wt% PVB, 45 wt% DMAc and 45 wt% ethanol were mixed in a 250 mL three-necked flask. The three-necked flask was placed in a 25 °C water bath and stirred for 12 h to obtain a uniform colorless and transparent casting solution. The casting solution was then allowed to stand for 12 h to remove bubbles, resulting in a 10 wt% PVB coating solution.
[0080] (3) Preparation of alkali-resistant flat-sheet PVDF membrane
[0081] The doctor blade height of the automatic film coating machine was adjusted to 0.320 mm, and the coating speed was 3 m / min. A 5 wt% PVE coating solution was poured onto a glass plate coated with a wet PVDF flat sheet film and coated. The film was then left to stand in the air for at least 1 minute to allow the coating solution to penetrate. A 10 wt% PVB coating solution was then poured onto the glass plate for a second coating and coating process to obtain the nascent composite film. The nascent composite film was slowly immersed in a room temperature water coagulation bath for further film formation. After removing the film from the coagulation bath, it was soaked in clean room temperature water for 48 hours to remove residual solvent. The film was then transferred to a room temperature glycerol aqueous solution and soaked for 48 hours. Finally, the film was air-dried to obtain a PVDF-based alkali-resistant water-treated flat sheet film.
[0082] Example 4
[0083] This embodiment provides an alkali-resistant flat-sheet PVDF membrane and its preparation method, specifically including the following steps:
[0084] (1) Preparation of flat PVDF base film
[0085] 14 wt% PVDF, 2 wt% PVP, and 84 wt% DMAc were mixed in a 250 mL three-necked flask. The flask was placed in a 90 °C oil bath and stirred for 12 h to obtain a uniform, pale yellow, transparent casting solution. The casting solution was then transferred to a 70 °C oil bath and allowed to stand for 12 h to degas. The degassed casting solution was poured onto a glass plate heated to 50 °C and covered with nonwoven fabric. The height of the doctor blade of the automatic film scraper was adjusted to 0.400 mm, and the film was scraped at a speed of 3 m / min to obtain an unseparated PVDF primary base film.
[0086] The unseparated PVDF nascent base membrane was immersed in a pure water coagulation bath at 25°C for further membrane formation. The resulting membrane was then soaked in clean room temperature water for 48 hours to remove residual DMAc. The membrane was then removed and the surface moisture was wiped dry with filter paper to obtain a wet flat sheet PVDF base membrane.
[0087] (2) Preparation of modified coating solution
[0088] 5 wt% PVE, 40 wt% DMAc and 60 wt% ethanol were mixed in a 250 mL three-necked flask. The three-necked flask was placed in a 25 °C water bath and stirred for 12 h to obtain a uniform colorless and transparent casting solution. The casting solution was then allowed to stand for 12 h to remove bubbles, resulting in a 5 wt% PVE coating solution.
[0089] 10 wt% PVE, 45 wt% DMAc and 45 wt% ethanol were mixed in a 250 mL three-necked flask. The three-necked flask was placed in a 25 °C water bath and stirred for 12 h to obtain a uniform colorless and transparent casting solution. The casting solution was then allowed to stand for 12 h to remove bubbles, resulting in a 10 wt% PVE coating solution.
[0090] (3) Preparation of alkali-resistant flat-sheet PVDF membrane
[0091] The doctor blade height of the automatic film coating machine was adjusted to 0.320 mm, and the coating speed was 3 m / min. A 5 wt% PVE coating solution was poured onto a glass plate coated with a wet PVDF flat sheet film and coated. The film was then left to stand in the air for at least 1 minute to allow the coating solution to penetrate. A second coating of 10 wt% PVE solution was then poured onto the glass plate to obtain the nascent composite film. The nascent composite film was slowly immersed in a room temperature water coagulation bath for further film formation. After removing the film from the coagulation bath, it was soaked in clean room temperature water for 48 hours to remove residual solvent. The film was then transferred to a room temperature glycerol aqueous solution and soaked for 48 hours. Finally, the film was air-dried to obtain a PVDF-based alkali-resistant water-treated flat sheet film.
[0092] Dissolve 4g of NaOH in 100mL of deionized water and sonicate to obtain a 1M NaOH solution. Take a 2cm*2cm dry PVDF base membrane, a PVB membrane, a PVE membrane, and an alkali-resistant flat PVDF membrane prepared in Examples 1-4. Use a disposable dropper to drop 1M NaOH solution onto each membrane. To prevent the alkali solution from evaporating and affecting the observation, add more drops after 1 hour. Observe the color change of the membrane within 2 hours. The results are as follows. Figure 6 As shown.
[0093] observe Figure 6 It can be seen that the PVDF-based film gradually turns yellow after NaOH is added, indicating that the PVDF has been corroded. The color change is due to the C=C bonds formed by the defluorination of hydrogen in the PVDF polymer chain, and the darker the color, the more complete the defluorination.
[0094] The pure PVB and PVE films showed no change in color over time, and no peeling or other changes were observed, indicating that PVB and PVE are resistant to alkali corrosion.
[0095] Examples 1 and 2 describe membranes prepared by simultaneous coating. PVB and PVE were coated onto an unseparated nascent PVDF substrate membrane before coagulation. After adding alkali solution, the solution penetrated the membrane over time, resulting in a faint yellow tinge on the membrane surface. This indicates that the PVB and PVE coating protected the PVDF substrate membrane and reduced the corrosive effect of the alkali on PVDF. The rapid alkali penetration rate is due to two factors: first, although the pore size of the alkali-resistant flat-sheet PVDF membranes prepared in Examples 1 and 2 is smaller than that of the substrate membrane, they are still relatively porous, resulting in low permeation resistance; second, the coating with PVB and PVE increases the membrane's hydrophilicity (reflected in...). Figure 7 (The contact angle changes significantly, which is beneficial for the penetration of the coating liquid.)
[0096] In Examples 3 and 4, the PVDF-based alkali-resistant water treatment membranes were prepared by stepwise coating. Specifically, after coating a wet PVDF base membrane with PVB and PVE, the membrane was then placed in a coagulation bath to allow the coating layer to separate into phases. After the addition of alkali solution, the membrane surface showed no color change over time. This is because the phase-separated base membrane hinders the exchange of solvent and water during phase separation in the coating layer, delaying phase separation and making the surface denser, thus impeding alkali penetration. Furthermore, the results of Examples 3 and 4 also demonstrate that coating with PVB and PVE effectively prevents the PVDF base membrane from being exposed to alkali solution, providing protection.
[0097] The embodiments of this application have been described above with reference to the accompanying drawings. However, this application is not limited to the specific embodiments described above. The specific embodiments described above are merely illustrative and not restrictive. Those skilled in the art can make many other forms under the guidance of this application without departing from the spirit and scope of the claims, and all of these forms are within the protection scope of this application.
Claims
1. A method for preparing an alkali-resistant polymer MBR membrane, characterized in that, The process includes the following steps: Step S1, preparing a polymer MBR base membrane with a cross-section of interpenetrating network or finger pores; Step S2: Prepare two modified coating solutions with different concentrations. The modified coating solutions are prepared by dissolving alkali-resistant viscous coating polyvinyl acetal in a second solvent. Step S3: The two modified coating solutions are applied to the surface of the polymer MBR base membrane in multiple applications to form an alkali-resistant coating, wherein the application of the low-concentration modified coating solution is performed before that of the high-concentration modified coating solution. The polymer MBR base membrane is an unseparated primary base membrane or a wet membrane obtained after the primary base membrane is separated into phases in a room temperature water coagulation bath. The thickness of the polymer MBR base membrane is 0.240-0.270 mm. The time interval between applying the two modified coating solutions shall not be less than 1 minute.
2. The preparation method according to claim 1, characterized in that, The preparation process of the unseparated primary base film specifically includes the following steps: Step S11: According to the mass fraction, 14% of the polymer, 1%-5% of the pore-forming agent and 81%-85% of the first solvent are added to a three-necked flask and mixed. The temperature is raised to 80-90℃ and stirred for 12 h to obtain the casting solution. Step S12: The casting solution is allowed to stand at 70°C to degas, and then poured onto a glass plate heated to 50°C and covered with non-woven fabric to obtain an unseparated nascent base film. The wet membrane preparation process, in addition to the unseparated primary base membrane preparation process, also includes the following steps: Step S13: Immerse the unseparated nascent base membrane in a pure water coagulation bath at 25°C to further form a membrane. Soak the obtained membrane in clean room temperature water for 48 hours to remove the residual first solvent. Then take out the membrane and wipe the surface moisture with filter paper to obtain a wet membrane.
3. The preparation method according to claim 2, characterized in that, The pore-forming agent is selected from at least one of calcium chloride, polyvinylpyrrolidone, and polyethylene glycol; the polymer is selected from one of PVDF, PAN, and PVC; and the first solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, or N-methylpyrrolidone.
4. The preparation method according to claim 1, characterized in that, The adhesive coating is selected from at least one of polyvinyl alcohol formaldehyde, polyvinyl alcohol acetal, and polyvinyl alcohol butyral; the second solvent is selected from at least one of ethanol, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.
5. The preparation method according to claim 4, characterized in that, The two modified coating liquids contain viscous coatings with the same composition.
6. The preparation method according to claim 4, characterized in that, The two modified coating solutions have different compositions of viscous coatings.
7. The preparation method according to claim 5 or 6, characterized in that, In any of the modified coating solutions, the mass fraction of the viscous coating is 5%-10%.
8. An alkali-resistant polymer MBR membrane, characterized in that, The alkali-resistant polymer MBR membrane is prepared by the preparation method according to any one of claims 1-7, and the thickness of the membrane is 0.320 mm.
Citation Information
Patent Citations
Method for enhancing alkaline corrosion resistance of polyvinylidene fluoride
CN102382323A
Modification method of alkali-resistant PVDF material
CN111484639A
Method for preparing hydrophilic macromolecule microporous composite membrane
CN102614787A
A braided tube homogeneously-enhanced type polyvinylidene fluoride hollow fiber film and a preparing method thereof