Non-metal doped bismuth layer-structured oxide, method for preparing same, and use thereof

By preparing a honeycomb nanosheet array structure of non-metal-doped bismuth layered oxide, the problems of low reaction rate and narrow voltage window of CO₂ electrocatalytic hydrogenation were solved, and the effect of efficient electrocatalytic reduction of CO₂ to formic acid was achieved.

CN118026259BActive Publication Date: 2026-11-24BEIJING UNIV OF CHEM TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410203934.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-23
Publication Date
2026-11-24
Estimated Expiration
2044-02-23

AI Technical Summary

Technical Problem

Existing CO₂ electrocatalytic hydrogenation reactions suffer from low rates, low selectivity, and narrow voltage windows, limiting their practical applications.

Method used

A non-metal-doped bismuth layered oxide was prepared by forming a seed layer on a conductive substrate, followed by hydrothermal reaction and electrodeposition. This non-metal-doped bismuth oxide with a honeycomb nanosheet array structure was then used as an electrocatalyst for the electrocatalytic reduction of CO₂.

Benefits of technology

This improved the efficiency of electrocatalytic reduction of CO₂, expanded the voltage window, promoted the efficient conversion of CO₂ to formic acid, and provided a new approach for the preparation of high-value-added chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118026259B_ABST
    Figure CN118026259B_ABST
Patent Text Reader

Abstract

This invention discloses a non-metal-doped bismuth layered oxide, its preparation method, and its application. First, a pretreated conductive substrate is immersed in a bismuth precursor solution. A bismuth layered oxide with a honeycomb nanosheet array structure is synthesized on the conductive substrate via a hydrothermal method. Then, a non-metal is doped into the bismuth layered oxide structure via electrodeposition, resulting in a non-metal-doped bismuth layered oxide with a honeycomb nanosheet array structure supported on the conductive substrate. This non-metal-doped bismuth layered oxide can be applied in the electrocatalytic reduction of CO2. The heteroatom-doped bismuth layered oxide prepared by this invention has a more stable structure and improved performance. Its honeycomb nanosheet array structure provides a large electrochemical current density, making it suitable as a cathode catalyst in the electrocatalytic reduction of CO2, promoting high Faradaic efficiency for CO2 production over a wide voltage range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nanomaterial synthesis and application technology, specifically relating to a non-metal-doped bismuth oxide and its preparation method and application. Background Technology

[0002] The rapid development of modern industry has led to the massive emission of the greenhouse gas CO2 into the atmosphere in a short period, causing severe damage to the Earth's ecological environment and making global warming one of the most important problems facing humanity in the 21st century. To mitigate this problem, it is necessary not only to change existing energy consumption patterns but also to vigorously develop economically feasible technologies for capturing and converting CO2. Electrocatalytic conversion technology driven by renewable energy sources (such as solar and wind power) is currently a research hotspot. The electrocatalytic hydrogenation of CO2 to formic acid is an important industrial reaction. Formic acid has wide applications in the production of commercial chemicals such as leather, pharmaceuticals, rubber, and dyes, and can also be used in fuel cells.

[0003] To date, CO2 has been successfully electrocatalyzed to formic acid using relatively inexpensive metals (such as Bi, Sn, and In). However, current research still faces challenges such as low reaction rates, low selectivity, and narrow voltage windows for the target product due to multiple reaction pathways and competition from hydrogen evolution reactions, hindering its practical application. Therefore, finding catalysts with high activity and high selectivity for CO2ER remains a significant challenge. Summary of the Invention

[0004] This invention addresses the problem of narrow voltage windows for target products in the electrocatalytic hydrogenation of carbon dioxide in existing research. Its purpose is to provide a non-metal-doped bismuth oxide, its preparation method, and its application to improve the efficiency of electrocatalytic reduction of carbon dioxide.

[0005] This invention is achieved through the following technical solution: A method for preparing a non-metal-doped bismuth layered oxide includes the following steps: (i) Forming a seed layer on the pretreated conductive substrate; (ii) A conductive substrate forming a seed layer is placed in a high-pressure reactor containing a bismuth precursor solution and subjected to hydrothermal reaction to obtain a bismuth layered oxide. (iii) The conductive substrate with bismuth layered oxide loaded in step (ii) is immersed in a non-metallic ion salt solution, and non-metals are doped into the bismuth layered oxide structure by electrodeposition to obtain a non-metallic doped bismuth layered oxide with a honeycomb nanosheet array structure loaded on the conductive substrate.

[0006] In the above technical solution, the method for forming the seed layer is as follows: the pretreated conductive substrate is soaked in the sowing solution for 10 min to 30 min, and after soaking, it is taken out and dried at 50 ℃ to 70 ℃, and after drying, it is heated at 180 ℃ for 5 min; the soaking, drying and heating operations are repeated multiple times to obtain the conductive substrate forming the seed layer.

[0007] In the above technical solution, the preparation methods for the bismuth precursor solution and the seeding solution are the same, specifically: dissolving bismuth salt in ethylene glycol, stirring until fully dissolved to form a transparent solution, adding ethanol, and stirring until fully dissolved to obtain the bismuth precursor solution; the bismuth salt is any one or more of bismuth nitrate, bismuth chloride, or bismuth sulfate; the volume ratio of ethylene glycol to ethanol is 1:2 to 1:4; the concentration of bismuth salt in the seeding solution is 0.03 mol / L to 0.06 mol / L; the concentration of bismuth salt in the bismuth precursor solution is 0.03 mol / L to 0.05 mol / L. The seeding solution forms a seed layer on the conductive material but does not generate the substance itself, while the precursor solution allows the nanosheet-like structure of the substance to grow on the conductive substrate.

[0008] In the above technical solution, the conductive substrate is any one of carbon cloth, carbon paper, nickel foam, nickel sheet, copper mesh, copper sheet, copper foam, titanium mesh, stainless steel, iron sheet, or FTO conductive glass.

[0009] In the above technical solution, the pretreatment method of the conductive substrate is as follows: immerse the conductive substrate in a potassium permanganate solution with a concentration of 0.1M to 0.2M for 30 min to 60 min, and then take it out and wash it with deionized water.

[0010] In the above technical solution, the reaction conditions of the hydrothermal method are: reacting at a constant temperature of 140 ℃~180 ℃ for 4 h~8 h, then taking it out, rinsing it, and drying it at 60 ℃~80 ℃.

[0011] In the above technical solution, the non-metallic ion in step (ii) is any one or more of fluorine, chlorine, bromine, iodine, astatine, sulfur or phosphorus; the concentration of the non-metallic ion salt solution is 1.5 mol / L to 3 mol / L.

[0012] In the above technical solution, the conditions for the electrodeposition method are as follows: a conductive substrate loaded with bismuth oxide serves as the anode, a platinum electrode as the counter electrode, a saturated calomel electrode as the reference electrode, and the electrochemical deposition process is performed using cyclic voltammetry (CV) (voltage range: 0~2 V) at a scan rate of 100 mV s. -1 ~200mV s -1 Repeat 20 to 40 times.

[0013] A non-metal-doped bismuth layered oxide, wherein a non-metal is doped into a bismuth layered oxide nanosheet structure; the non-metal is any one or more of fluorine, chlorine, bromine, iodine, astatine, sulfur, or phosphorus; the particle size of the non-metal is in the range of 1 nm to 5 nm; the size of the nanosheet is 100 nm to 500 nm; the doping amount of the non-metal is 3% to 4% of the mass of the bismuth oxide, and both the bismuth layered oxide before and after doping have a honeycomb nanosheet array.

[0014] An application of a non-metal-doped bismuth layered oxide in the electrocatalytic reduction of CO2, wherein the non-metal-doped bismuth oxide supported on a conductive substrate serves as a cathode, and is assembled into an electrolytic cell with an anode and an electrolyte. CO2 is added to the electrolyte, and CO2 is electrocatalytically reduced to formic acid.

[0015] In the above technical solution, the electrolyte is a solution of any one or more of lithium hydroxide, potassium hydroxide, sodium hydroxide, potassium bicarbonate, potassium carbonate, sodium bicarbonate, sodium carbonate, sodium sulfate, or potassium sulfate; the electrolyte concentration is 0.4 M to 0.7 M; the CO2 concentration is 0.03 M to 0.05 M; the anode is an oxygen evolution catalyst supported on a conductive substrate, and the oxygen evolution catalyst is one or more of iridium / carbon catalyst, ruthenium / carbon catalyst, iridium dioxide, ruthenium dioxide, nickel-iron hydrotalcite, or nickel hydroxide.

[0016] In the above technical solution, the electrocatalytic conditions are electrocatalysis at a voltage of -0.67 V to -1.17 V vs. RHE on the cathode.

[0017] The beneficial effects of this invention are: This invention provides a non-metal-doped bismuth layered oxide, its preparation method, and its application. The prepared non-metal-doped bismuth oxide has a honeycomb nanosheet array structure, which provides a large electrochemical active area and can promote the enrichment of carbon dioxide on the electrode surface during electrocatalytic reduction reactions. Its tight bonding with the conductive substrate as a catalyst can accelerate electron transport and increase current density. The bismuth / heteroatom structure in the bismuth oxide can effectively regulate the charge distribution of the layers, improving the intrinsic activity of the catalyst. The non-metallic components in the bismuth oxide can promote the decomposition of water to produce H*, thereby promoting the hydrogenation reaction of carbon dioxide. This provides a novel catalyst for the efficient conversion and utilization of carbon dioxide to prepare high-value-added chemicals. It also generates a non-metal-doped bismuth oxide with improved performance, thus providing a new approach for the design and controllable preparation of bismuth-based nanomaterials. Attached Figure Description

[0018] Figure 1 This is a SEM image of the carbon cloth-supported bismuth oxide prepared in Example 1 of this invention; Figure 2This is a SEM image of the carbon cloth loaded with fluorine-doped bismuth oxide prepared in Example 1 of this invention; Figure 3 This is a TEM image of the carbon cloth-supported fluorine-doped bismuth oxide prepared in Example 1 of this invention; Figure 4 These are the XRD patterns of carbon cloth-supported bismuth oxide and carbon cloth-supported fluorine-doped bismuth oxide prepared in Example 1 of this invention. Figure 5 This is a graph showing the electrochemical (time-current) test data of CO2 hydrogenation in Example 1 of this invention; Figure 6 These are the Faradaic efficiency results of the formic acid products prepared by electrocatalytic CO2 hydrogenation in Example 1 and Comparative Example 1 of this invention;

[0019] Figure 7 These are the Faradaic efficiency results of the formic acid products prepared by long-term electrocatalytic CO2 hydrogenation in Example 1 and Comparative Example 2 of this invention;

[0020] For those skilled in the art, other related figures can be obtained from the above figures without any creative effort. Detailed Implementation

[0021] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments. Example 1

[0022] (I) Synthesis of fluorine-doped bismuth oxide supported on carbon paper (nanosheet array electrode): (i) Soak appropriately cut carbon paper in 0.15 M (mol / L) potassium permanganate solution for half an hour, then take it out, wash it with deionized water and dry it. (ii) Prepare the sowing solution Dissolve 97 mg Bi(NO)3·5H2O in 13.72 mL of ethylene glycol, stir at room temperature for 10 min to form a clear solution, add 26.8 mL of ethanol, and continue stirring for 10 min. The concentration of Bi(NO)3·5H2O is 0.005 mol / L; (iii) Preparation of bismuth precursor solution: Dissolve 3.88 gBi(NO)3·5H2O in 68 mL of ethylene glycol, stir at room temperature for 10 min to form a transparent solution, add 136 mL of ethanol, and continue stirring for 10 min. The concentration of Bi(NO)3·5H2O is 0.04 mol / L; (iv) Formation of the seed layer The carbon paper was soaked in the above seeding solution for 2 hours. After soaking, the carbon paper was removed and dried in an oven at 60 °C for 10 minutes. Then it was heated in an oven at 180 °C for 5 minutes to form a seed layer. In order to better disperse the seeds, step (iv) was repeated multiple times to finally obtain a conductive substrate loaded with a seed layer. (v) Hydrothermal reaction The conductive substrate loaded with the seed layer was immersed in a high-pressure reactor containing a bismuth precursor solution. After hydrothermal growth at 160 °C for 5 h, the carbon paper was removed, rinsed with water and ethanol to remove other residues, and dried at 60 °C to obtain carbon paper loaded with bismuth oxide. The SEM image of the prepared carbon paper-supported fluorine-doped bismuth oxide (nanosheet array electrode) is as follows: Figure 1 As shown, from Figure 1 It can be seen that the bismuth oxide on the carbon paper has a uniform sheet-like array structure; The XRD characterization results of the carbon paper-supported bismuth oxide are as follows: Figure 4 As shown, the catalyst used in its synthesis is bismuth oxycarbonate; (vi) Electrodeposition doping The carbon paper-supported bismuth oxide nanosheet array prepared in step (v) was immersed in a 2 M NH4F solution and fluorine-doped bismuth oxide was obtained by electrodeposition.

[0023] The electrodeposition conditions were as follows: carbon paper loaded with bismuth oxide was used as the anode, a platinum electrode as the counter electrode, and a saturated calomel electrode as the reference electrode. The electrochemical activation process was performed using cyclic voltammetry (CV) (voltage range: 0~2 V) at a scan rate of 100 mV / s. -1 Repeat 40 times; The SEM image of the prepared carbon paper-supported fluorine-doped bismuth oxide (nanosheet array electrode) is as follows: Figure 2 As shown, from Figure 2 It can be seen that the carbon paper-loaded fluorine-doped bismuth oxide has a uniform sheet-like array structure, which is not significantly different from the morphology of undoped tin oxide. TEM images of the carbon paper-supported fluorine-doped bismuth oxide (nanosheet array electrode) are as follows: Figure 3 As shown, from Figure 3 It can be seen that the nanoscale size of fluorine-doped bismuth oxide loaded on carbon paper is 5 nm; The XRD characterization results of the carbon paper-supported fluorine-doped bismuth oxide are as follows: Figure 4 As shown, F doping can be incorporated into the catalyst structure to form BiO. 0.51 F 1.98 This distinguishes it from Bi2O3CO3, proving that the catalyst used in its synthesis is fluorine-doped bismuth oxide; (II) Using carbon paper loaded with fluorine-doped layered bismuth oxide (nanosheet array electrode) for the preparation of formic acid by CO2 hydrogenation: (i) A three-electrode system was constructed using the prepared carbon paper-supported fluorine-doped bismuth oxide (nanosheet array) as the cathode, the conductive substrate supporting the oxygen evolution catalyst as the anode, the platinum sheet as the counter electrode, and the Ag / AgCl electrode as the reference electrode; the oxygen evolution catalyst used in the anode was cobalt-nickel hydrotalcite. (ii) During the electrochemical performance test, a 0.5 M potassium bicarbonate solution was used as the electrolyte solution, and the reaction was carried out at a voltage of −0.87 V vs. RHE for 1 h. (iii) Perform liquid phase analysis on the solution after the reaction to determine the products.

[0024] The electrochemical (time-current) test of CO2 hydrogenation is as follows: Figure 5 As shown, from Figure 5 It can be seen that carbon paper loaded with fluorine-doped bismuth oxide has a large current density and excellent stability.

[0025] The Faradaic efficiency results of the formic acid product obtained by electrocatalytic CO2 hydrogenation are as follows: Figure 6 As shown. From Figure 6 It can be seen that the performic acid exhibits a Faraday efficiency of >90% within a wide potential window of −0.77 V to −1.17 V vs. RHE. Example 2

[0026] (I) Synthesis of nickel foam supported sulfur-doped bismuth oxide (nanosheet array electrode) (i) Wash the appropriately cut nickel foam in ethanol, 35% dilute sulfuric acid solution, and deionized water for 30 minutes each, then remove and dry. (ii) Prepare the sowing solution Dissolve 97 mg Bi(NO)3·5H2O in 13.72 mL of ethylene glycol, stir at room temperature for 10 min to form a clear solution, add 26.8 mL of ethanol, and continue stirring for 10 min. The concentration of Bi(NO)3·5H2O is 0.005 mol / L; (iii) Preparation of bismuth precursor solution: Bi(NO)3·5H2O was dissolved in 68 mL of ethylene glycol, with a concentration of 0.04 mol / L. The solution was stirred at room temperature for 10 min to form a transparent solution. 136 mL of ethanol was added, and the mixture was stirred for another 10 min to obtain a bismuth precursor solution. (iv) Formation of the seed layer The carbon paper was soaked in the above seeding solution for 2 hours. After soaking, the carbon paper was removed and dried in an oven at 60 °C for 10 minutes. Then it was heated in an oven at 180 °C for 5 minutes to form a seed layer. In order to better disperse the seeds, step (iv) was repeated multiple times to finally obtain a conductive substrate loaded with a seed layer. Step (iv) is repeated multiple times to finally obtain a nickel foam-loaded seed layer; (v) Hydrothermal reaction The nickel foam forming the seed layer was immersed in a high-pressure reactor containing a bismuth precursor solution. After hydrothermal growth at 160 °C for 20 h, the nickel foam was removed, rinsed with water and ethanol to remove other residues, and dried at 80 °C to obtain bismuth oxide supported on nickel foam. (vi) Electrodeposition doping Thiourea was dissolved in 80 mL of ethylene glycol at room temperature with stirring. The concentration of thiourea was 0.03 mol / L. Then, the bismuth oxide foamed nickel supported by step (v) was immersed in a high-pressure reactor containing thiourea ethylene glycol solution and hydrothermally grown at 80 °C for 3 h to obtain bismuth oxide foamed nickel supported by sulfur doping. (II) Nickel foam supported on sulfur-doped bismuth oxide (nanosheet array electrode) for CO2 reduction to prepare formic acid: (i) A three-electrode system was constructed using the prepared nickel foam supported sulfur-doped bismuth oxide (nanosheet array electrode) as the cathode, a platinum sheet as the counter electrode, and an Ag / AgCl electrode as the reference electrode. The oxygen evolution catalyst used in the anode was cobalt-nickel hydrotalcite.

[0027] (ii) During the electrochemical performance test, a 0.5 M sodium bicarbonate solution was used as the electrolyte solution, and the reaction was carried out at a voltage of −0.87 V vs. RHE for 1 h.

[0028] (iii) Perform liquid phase analysis on the solution after the reaction to determine the products.

[0029] The formic acid product prepared by the electrocatalytic CO2 hydrogenation can achieve a Faraday efficiency of 85%. Example 3

[0030] (I) Synthesis of phosphorus-doped bismuth oxide supported on carbon cloth (nanosheet array electrode): (i) Soak the appropriately cut carbon cloth in a 0.15 M potassium permanganate solution for 30 min, take it out, wash it with deionized water and dry it; (ii) Prepare the sowing solution Dissolve 97 mg Bi(NO)3·5H2O in 13.72 mL of ethylene glycol, stir at room temperature for 10 min to form a clear solution, add 26.8 mL of ethanol, and continue stirring for 10 min. The concentration of Bi(NO)3·5H2O is 0.005 mol / L; (iii) Preparation of bismuth precursor solution: Bi(NO)3·5H2O was dissolved in 68 mL of ethylene glycol, and the concentration of Bi(NO)3·5H2O in the ethylene glycol was 0.04 mol / L. The mixture was stirred at room temperature for 10 min to form a transparent solution. 136 mL of ethanol was added and the mixture was stirred for another 10 min to obtain a bismuth precursor solution. (iv) Formation of the seed layer The carbon paper was soaked in the above seeding solution for 2 hours. After soaking, the carbon paper was removed and dried in an oven at 60 °C for 10 minutes. Then it was heated in an oven at 180 °C for 5 minutes to form a seed layer. In order to better disperse the seeds, step (iv) was repeated multiple times to finally obtain a conductive substrate loaded with a seed layer. (v) Hydrothermal reaction The carbon cloth forming the seed layer was immersed in a high-pressure reactor containing a bismuth precursor solution. After hydrothermal growth at 160 °C for 20 h, the carbon cloth was removed, rinsed with water and ethanol to remove other residues, and dried at 60 °C to obtain bismuth oxide loaded on the carbon cloth. (vi) Electrodeposition doping The carbon cloth-supported bismuth oxide precursor and NaH2PO2 obtained in step (v) were placed in two different positions in the quartz furnace of the tube furnace, and then heated to 350 °C in argon at a heating rate of 4 °C / min for 2 h. Finally, after cooling in the furnace, the carbon cloth-supported phosphorus-doped bismuth oxide was obtained. (II) Carbon cloth-supported phosphorus-doped bismuth oxide nanosheet array electrode for electrocatalytic CO2 hydrogenation to formic acid: (i) A three-electrode system was constructed using the prepared carbon cloth-supported phosphorus-doped bismuth oxide nanosheet array (catalyst) as the cathode, a platinum sheet as the counter electrode, and an Ag / AgCl electrode as the reference electrode. The oxygen evolution catalyst used at the anode was cobalt-nickel hydrotalcite. (ii) During the electrochemical performance test, a 0.5 M (mol / L) potassium bicarbonate solution was used as the electrolyte solution, and the reaction was carried out at a voltage of −0.87 V vs. RHE for 1 h. (iii) Perform liquid phase analysis on the solution after the reaction to determine the products.

[0031] The formic acid product prepared by the electrocatalytic CO2 hydrogenation can achieve a Faraday efficiency of over 85%.

[0032] Comparative Example 1 (Undoped) (i) Using the carbon paper-supported bismuth oxide (nanosheet array) prepared in Example 1 as the cathode, a platinum sheet as the counter electrode, and an Ag / AgCl electrode as the reference electrode, a three-electrode system was constructed; the conductive substrate supporting the oxygen evolution catalyst was used as the anode, and the oxygen evolution catalyst used in the anode was cobalt-nickel hydrotalcite.

[0033] (ii) During the electrochemical performance test, a 0.5 M potassium bicarbonate solution was used as the electrolyte solution, and the reaction was carried out for 1 h at a voltage of −0.67 V vs. RHE to −1.17 V vs. RHE.

[0034] (iii) Perform liquid phase analysis on the solution after the reaction to determine the products.

[0035] The Faradaic efficiency results of the formic acid product obtained by electrocatalytic CO2 hydrogenation are as follows: Figure 6 As shown. From Figure 6 It can be seen that the Faraday efficiency of formic acid is low under both low and high voltage conditions.

[0036] Comparative Example 2 (Doped Metal) (I) Synthesis of carbon paper-supported silver-doped bismuth oxide (nanosheet array electrode): (i) Soak appropriately cut carbon paper in 0.15 M (mol / L) potassium permanganate solution for half an hour, then take it out, wash it with deionized water and dry it. (ii) Prepare the sowing solution Dissolve 97 mg Bi(NO)3·5H2O in 13.72 mL of ethylene glycol, stir at room temperature for 10-30 min to form a clear solution, add 26.8 mL of ethanol, and continue stirring for 10-30 min. The concentration of Bi(NO)3·5H2O is 0.005 mol / L; (iii) Preparation of bismuth precursor solution: Dissolve AgCl and Bi(NO)3·5H2O in 68 mL of ethylene glycol, stir at room temperature for 10 min to 30 min to form a clear solution, add 136 mL of ethanol, and continue stirring for 10 min to 30 min. The concentration of AgCl is 0.01 mol / L to 0.1 mol / L, and the concentration of Bi(NO)3·5H2O is 0.04 mol / L; (iv) Formation of seeds The carbon paper was soaked in the above seeding solution for 2 hours. After soaking, the carbon paper was removed and dried in a 60° oven for 10 minutes. Then it was heated in a 180° oven for 5 minutes to form Bi2O3 seeds. In order to better disperse the Bi2O3 seeds, step (iv) was repeated multiple times to finally obtain Bi2O3 seeds loaded on a conductive substrate. (v) Hydrothermal reaction The conductive substrate loaded with Bi2O3 seeds was immersed in a high-pressure reactor containing a solution of silver and bismuth precursors. After hydrothermal growth at 160°C for 5 h, the carbon paper was removed, rinsed with water and ethanol to remove other residues, and dried at 60°C to obtain carbon paper loaded with silver-doped bismuth oxide. (II) Using carbon paper-supported silver-doped layered bismuth oxide (nanosheet array electrode) for the preparation of formic acid by CO2 hydrogenation: (i) A three-electrode system was constructed using the prepared carbon paper-supported silver-doped bismuth oxide (nanosheet array) as the cathode, the conductive substrate supporting the oxygen evolution catalyst as the anode, the platinum sheet as the counter electrode, and the Ag / AgCl electrode as the reference electrode; the oxygen evolution catalyst used in the anode was cobalt-nickel hydrotalcite.

[0037] (ii) During the electrochemical performance test, a 0.5 M potassium bicarbonate solution was used as the electrolyte solution, and the reaction was carried out at a voltage of −0.97 V vs. RHE for 20 h.

[0038] (iii) Perform liquid phase analysis on the solution after the reaction to determine the products.

[0039] The electrochemical test of CO2 hydrogenation is as follows: Figure 7 As shown, from Figure 7 It can be seen that the Faraday efficiency of carbon paper-supported fluorine-doped bismuth oxide is higher than that of carbon paper-supported silver-doped bismuth oxide within a reaction time of 30 h, while carbon paper-supported fluorine-doped bismuth oxide has excellent stability.

[0040] The reaction principle of this invention (taking Example 1 as an example): This invention constructs a carbon paper-supported fluorine-doped bismuth oxide (nanosheet array electrode) as the cathode electrocatalyst, using hydrogen / oxygen atoms in water as the source of [H] / [O] in the redox reaction. During the electrolysis of water, [H] is generated, and [H] undergoes electrocatalytic hydrogenation with C=O in CO2 to produce formic acid.

[0041] At the same time, water is oxidized into oxygen at the anode.

[0042] The reaction equation is:

[0043] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A method for preparing a non-metal-doped bismuth layer-oxide having a honeycomb-like nanosheet array structure supported on a conductive substrate, characterized by: The method comprises the following steps: (i) forming a seed layer on the pretreated conductive substrate; The pretreatment method of the conductive substrate is: soaking the conductive substrate in a potassium permanganate solution with a concentration of 0.1 M-0.2 M for 30 min-60 min, and then taking it out and washing it with deionized water; The forming method of the seed layer is: soaking the pretreated conductive substrate in a seeding solution for 10 min-30 min, taking it out and drying it at 50 ℃-70 ℃ after soaking, and then heating it at 180 ℃ for 5 min after drying; the seed layer forming conductive substrate is obtained after repeating the soaking, drying and heating treatment operations multiple times; (ii) placing the seed layer forming conductive substrate in a high-pressure reaction kettle containing a bismuth precursor solution to perform hydrothermal reaction to obtain a bismuth layered oxide; The configuration method of the bismuth precursor solution and the seeding solution is the same, specifically: dissolving bismuth salt in ethylene glycol, stirring until fully dissolved to form a transparent solution, adding ethanol, and stirring until fully dissolved to obtain the solution; The volume ratio of ethylene glycol to ethanol is 1:2-1:4; The concentration of bismuth salt in the seeding solution is 0.03 mol / L-0.06 mol / L; The concentration of bismuth salt in the bismuth precursor solution is 0.03 mol / L-0.05 mol / L; The reaction conditions of the hydrothermal reaction are: reacting at a constant temperature of 140 ℃-180 ℃ for 4 h-8 h, taking it out, rinsing and drying at 60 ℃-80 ℃; (iii) soaking the bismuth layered oxide loaded conductive substrate obtained in step (ii) in a non-metallic ion salt solution, doping non-metals into the bismuth layered oxide structure by electrodeposition to obtain a non-metallic doped bismuth layered oxide with a honeycomb-like nanosheet array structure loaded on the conductive substrate; The conditions of the electrodeposition method are as follows: the conductive substrate loaded with bismuth oxide as an anode, a platinum electrode as a counter electrode, a saturated calomel electrode as a reference electrode, the electrochemical deposition process is carried out by cyclic voltammetry, the scanning rate is 100 mV s -1 ~200 mV s -1 , and the cycle is 20~40 times. The non-metallic element in the non-metallic ion salt solution is any one or more of fluorine, chlorine, bromine, iodine, sulfur or phosphorus; the concentration of the non-metallic ion salt solution is 1.5 mol / L-3 mol / L; The doping amount of the non-metallic element is 3%-4% of the mass of the bismuth layered oxide.

2. The method of claim 1, wherein: Prepared by the method of any one of claims 1 or 2; the non-metallic element is doped in the bismuth layered oxide nanosheet structure; the non-metallic element is any one or more of fluorine, chlorine, bromine, iodine, sulfur or phosphorus; the particle size of the non-metallic element ranges from 1 nm to 5 nm; the size of the nanosheet is 100 nm-500 nm; both the bismuth layered oxide before and after doping have a honeycomb-like nanosheet array.

3. A non-metal doped bismuth layer-oxide having a honeycomb-like nanosheet array structure supported on a conductive substrate, characterized in that: In the application of electrocatalytic reduction of CO2, the non-metallic doped bismuth layered oxide with a honeycomb-like nanosheet array structure loaded on the conductive substrate is used as a cathode, an electrolytic cell is assembled with an anode and an electrolyte, CO2 is added to the electrolyte, and electrocatalytic reduction of CO2 generates formic acid.

4. Use of the non-metal-doped bismuth layer-structured oxide having a honeycomb nanosheet array structure supported on a conductive substrate according to claim 3, characterized by: ​ 5. Use of a non-metal doped bismuth layer-structured oxide having a honeycomb nanosheet array structure supported on an electrically conductive substrate according to claim 4, characterized in that: The electrolyte is a solution of any one or more of lithium hydroxide, potassium hydroxide, sodium hydroxide, potassium bicarbonate, potassium carbonate, sodium bicarbonate, sodium carbonate, sodium sulfate, or potassium sulfate; the electrolyte concentration is 0.4 M to 0.7 M; the CO2 concentration is 0.03 M to 0.05 M; the anode is an oxygen evolution catalyst supported on a conductive substrate, and the oxygen evolution catalyst is one or more of iridium / carbon catalyst, ruthenium / carbon catalyst, iridium dioxide, ruthenium dioxide, nickel-iron hydrotalcite, or nickel hydroxide.

6. Use of a non-metal doped bismuth layer-structured oxide having a honeycomb-like nanosheet array structure supported on an electrically conductive substrate according to claim 4, characterized in that: The electrocatalytic conditions are electrocatalysis at the cathode at a voltage of –0.67 V to –1.17 V vs. RHE.

Citation Information

Patent Citations

  • Bismuth-based catalyst for electrocatalytic CO2 reduction to form formic acid and preparation method and application thereof

    CN109518222A

  • Preparation method of metal-doped bismuth layered oxide and application of metal-doped bismuth layered oxide in electrocatalytic reduction of CO2

    CN113828300A

  • Bismuth-based catalyst as well as preparation method and application thereof

    CN117364144A