Sodium-ion battery precursor and preparation method thereof, sodium-ion battery positive electrode material and preparation method thereof

By designing a gradient distribution of nickel and manganese in the sodium-ion battery precursor and employing gradient temperature sintering technology, the problems of uneven concentration and stability of the cathode material in sodium-ion batteries were solved, thereby improving the electrochemical performance and lifespan of the battery.

CN118026282BActive Publication Date: 2026-11-20陕西红马科技有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410096583.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-23
Publication Date
2026-11-20
Estimated Expiration
2044-01-23

AI Technical Summary

Technical Problem

Existing sodium-ion battery cathode materials suffer from uneven concentration gradient distribution and poor cycle stability, which affect their electrochemical performance and lifespan.

Method used

A sodium-ion battery precursor was designed with nickel and manganese content distributed in a radial gradient. By precisely controlling the addition of nickel and manganese salts, a sodium-ion battery cathode material with uniform chemical composition was prepared. A gradient temperature sintering technique was used to form a concentration gradient distribution.

Benefits of technology

It improves the cycle stability and structural stability of sodium-ion battery cathode materials, enhances discharge specific capacity and rate performance, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118026282B_ABST
    Figure CN118026282B_ABST
Patent Text Reader

Abstract

This invention relates to the field of sodium-ion battery technology, and discloses a sodium-ion battery precursor and its preparation method, as well as a sodium-ion battery cathode material and its preparation method. The sodium-ion battery precursor is spherical and / or near-spherical in shape, and comprises nickel, manganese, and M metal. The contents of nickel and manganese are distributed in a radial gradient; the nickel content decreases gradient from the center of the sphere to the outer surface, and the manganese content increases gradient from the center of the sphere to the outer surface; the particle size D of the sodium-ion battery precursor is... 50 The content of nickel and manganese in the sodium-ion battery precursor is 2-15 μm. In this invention, nickel salt solution, manganese salt solution and M salt solution are added to carry out co-precipitation reaction, and the flow rates of the added nickel salt solution and manganese salt solution vary according to the corresponding formula. The content of nickel and manganese in the prepared sodium-ion battery precursor is linearly distributed in the radial direction, and the obtained sodium-ion battery cathode material has excellent cycle stability and rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium-ion battery technology, specifically to a sodium-ion battery precursor and its preparation method, and a sodium-ion battery cathode material and its preparation method. Background Technology

[0002] The ever-expanding demand for lithium-ion batteries will also face the problem of raw material shortages. Therefore, sodium metal, which is abundant and has similar properties to lithium metal, has broad prospects in the field of energy storage.

[0003] However, the large sodium ion radius, slow electrochemical kinetics, and other related issues have become major obstacles to the development of electrodes suitable for high-performance sodium-ion batteries (SIBs). As a crucial component of SIBs, the cathode material significantly impacts their electrochemical performance; therefore, the development of high-performance cathode materials is key to improving the energy density of SIBs and promoting their commercialization. Currently, layered sodium transition metal oxides possess a simple structure, and the redox reaction based on lattice oxygen (oxygen valence variation) has been shown to significantly enhance the specific capacity of cathode materials, offering numerous advantages. Furthermore, their ease of synthesis has led them to stand out among various sodium-ion battery cathode materials, gaining widespread application and becoming a key area of ​​focus for sodium-ion battery cathode materials. However, these oxygen valence variation materials often exhibit poor reversibility and capacity decay, severely limiting their practical applications.

[0004] To address these issues, techniques such as doping and coating modification are used to regulate the redox reaction of lattice oxygen. Specifically, layered transition metal oxide cathodes in sodium-ion batteries suffer from low initial coulombic efficiency, structural disorder, voltage hysteresis, voltage drop, cycle instability, and low structural stability due to oxygen escape from the crystal caused by oxygen valence changes. High-capacity oxygen-valence-change cathode materials are difficult to meet practical applications. Furthermore, sodium-ion battery cathode materials without a concentration gradient and without gradient microstructure design suffer significant losses in cycle stability and rate performance. The dissolution of nickel ions in the electrolyte without a concentration gradient is severe; excessively high external nickel content can lead to dissolution reactions with the electrolyte, resulting in poor cycle life for normal layered oxides. Therefore, it is advisable to consider designing sodium-ion battery cathode materials with a gradually decreasing molar percentage of nickel from the inside out.

[0005] CN108565457A discloses a sodium-ion battery cathode material that involves directly mixing an alkaline solution and a mixed metal salt solution for a co-precipitation reaction. A manganese salt solution is added to the co-precipitation reaction system to obtain a mixed metal carbonate precipitate. This material is doped with manganese, nickel, and cobalt. Only manganese and nickel exhibit a concentration gradient, while cobalt does not. Furthermore, the method of adding manganese and nickel in the co-precipitation reaction cannot ensure a uniform distribution of the concentration gradient, easily leading to concentration aggregation regions, which is detrimental to the preparation of a qualified sodium-ion battery cathode material.

[0006] Therefore, the development of a sodium-ion battery cathode material with a concentration gradient distribution and high cycle stability is of great practical significance. Summary of the Invention

[0007] The purpose of this invention is to overcome the problems of uneven concentration gradient distribution and poor cycle stability in existing sodium-ion battery cathode materials, and to provide a sodium-ion battery precursor and its preparation method, as well as a sodium-ion battery cathode material and its preparation method. The chemical composition of this sodium-ion battery cathode material exhibits a uniform concentration gradient distribution, thereby improving the cycle stability and rate performance of the cathode material.

[0008] To achieve the above objectives, the first aspect of the present invention provides a sodium-ion battery precursor, wherein the sodium-ion battery precursor is spherical and / or near-spherical in shape, and the sodium-ion battery precursor comprises nickel, manganese, and M metal, wherein the contents of nickel and manganese are distributed in a radial gradient; M is selected from at least one of Fe, Mg, Al, Ti, W, Cu, and Co.

[0009] Among them, the nickel content decreases in a gradient from the center of the sphere to the outer surface, while the manganese content increases in a gradient from the center of the sphere to the outer surface.

[0010] Based on the total amount of nickel, manganese and M metal in the innermost layer, the nickel content in the innermost layer is 45-80 mol%, and the manganese content in the innermost layer is 0-30 mol%.

[0011] Based on the total amount of nickel, manganese and M metal in the outermost layer, the content of nickel in the outermost layer is 10-40 mol%, and the content of manganese in the outermost layer is 35-70 mol%.

[0012] Wherein, the particle size D of the sodium-ion battery precursor 50 It is 2-15μm.

[0013] A second aspect of the present invention provides a method for preparing a sodium-ion battery precursor, wherein the method includes the following steps:

[0014] (1) Prepare nickel salt solution, manganese salt solution, M salt solution, precipitant solution and complexing agent solution respectively;

[0015] (2) Mix the precipitant solution, complexing agent solution and water to prepare the bottom liquid of the reaction vessel;

[0016] (3) Add nickel salt solution, manganese salt solution, M salt solution, precipitant solution and complexing agent solution to the bottom liquid of the reaction vessel at the same time and react to obtain a solid-liquid mixed slurry;

[0017] (4) The solid-liquid mixture is washed, dried and sieved to obtain the sodium-ion battery precursor;

[0018] Wherein, M is selected from at least one of Fe, Mg, Al, Ti, W, Cu and Co;

[0019] The flow rate of the added nickel salt solution is determined according to formula Q. Ni =S Ni +n Ni αt changes, where Q Ni S is the instantaneous flow rate of the nickel salt solution. Ni n is the initial flow rate of the nickel salt solution. Ni Let be the molar concentration of the nickel salt solution, α be the flow rate coefficient of the nickel salt solution, -0.02≤α≤-0.15, and t be the reaction time;

[0020] The flow rate of the added manganese salt solution is determined according to formula Q. Mn =S Mn +n Mn βt change, where Q Mn S is the instantaneous flow rate of the manganese salt solution. Mn Let n be the initial flow rate of the manganese salt solution. Mn denoted as ωm, where ω is the molar concentration of the manganese salt solution, β is the flow rate variation coefficient of the manganese salt solution (0.02 ≤ β ≤ 0.15), and t is the reaction time.

[0021] The third aspect of the present invention provides a sodium-ion battery cathode material, wherein the cathode material is obtained by gradient temperature sintering of a sodium-ion battery precursor prepared by the method described in the first aspect or the method described in the second aspect above with a sodium source.

[0022] A fourth aspect of the present invention provides a method for preparing the sodium-ion battery cathode material described in the third aspect above, wherein the method includes:

[0023] The sodium-ion battery precursor and sodium source are mixed and then subjected to gradient temperature sintering to obtain the cathode material.

[0024] Through the above technical solution, the present invention has the following beneficial effects:

[0025] (1) The sodium-ion battery precursor provided by the present invention has a chemical composition that is uniformly distributed in a gradient and has no internal discontinuities and is tightly connected. The molar percentage of nickel decreases from the center of the sphere to the outer surface, while the molar percentage of manganese increases. This gradient structure is beneficial for buffering the volume change of the core of the prepared sodium-ion battery cathode material during charging and discharging, reducing structural collapse during repeated charging and discharging, and improving the cycle stability and structural stability of the cathode material. Its innermost layer is rich in nickel and its outermost layer is rich in manganese, which improves the discharge specific capacity and long-term cycle stability. Its processing performance and safety performance are also significantly improved.

[0026] (2) The sodium-ion battery precursor provided by the present invention feeds nickel salt, manganese salt and M salt solution through a precision flow pump and a precision mass flow meter. The nickel salt and manganese salt are fed according to the corresponding flow rate change formula. Compared with the existing sodium-ion battery cathode material with uniform internal structure, the gradient distribution sodium-ion battery cathode material has a higher discharge specific capacity, improves the cycle stability, high temperature cycle stability and rate performance of the sodium-ion battery cathode material, and improves the precise control of the content of manganese, nickel and M metal in the sodium-ion battery precursor. It has strong operability, excellent processing performance and can be used for industrial production. Attached Figure Description

[0027] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the following detailed description to explain the invention, but do not constitute a limitation thereof.

[0028] Figure 1 This is a schematic diagram of the preparation process of the sodium-ion battery precursor and its cathode material according to the present invention;

[0029] Figure 2 This is an elemental distribution diagram of the sodium-ion battery precursor of Embodiment 1 of the present invention;

[0030] Figure 3 This is an elemental distribution diagram of the sodium-ion battery precursor of Embodiment 2 of the present invention;

[0031] Figure 4 This is an elemental distribution diagram of the sodium-ion battery precursor of Embodiment 3 of the present invention;

[0032] Figure 5 This is an elemental distribution diagram of the sodium-ion battery precursor of Comparative Example 1 of this invention;

[0033] Figure 6 This is a comparison chart of the cycle performance of batteries prepared with positive electrode materials from Examples 1-3 and Comparative Example 2 at 25°C. Detailed Implementation

[0034] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0035] The first aspect of the present invention provides a sodium-ion battery precursor, wherein the sodium-ion battery precursor is spherical and / or near-spherical in shape, and the sodium-ion battery precursor includes nickel, manganese and M metal, wherein the contents of nickel and manganese are distributed in a radial gradient; M is selected from at least one of Fe, Mg, Al, Ti, W, Cu and Co;

[0036] Among them, the nickel content decreases in a gradient from the center of the sphere to the outer surface, while the manganese content increases in a gradient from the center of the sphere to the outer surface.

[0037] Based on the total amount of nickel, manganese and M metal in the innermost layer, the nickel content in the innermost layer is 45-80 mol%, and the manganese content in the innermost layer is 0-30 mol%.

[0038] Based on the total amount of nickel, manganese and M metal in the outermost layer, the content of nickel in the outermost layer is 10-40 mol%, and the content of manganese in the outermost layer is 35-70 mol%.

[0039] Wherein, the particle size D of the sodium-ion battery precursor 50 It is 2-15μm.

[0040] In this invention, the nickel and manganese content in the sodium-ion battery precursor is distributed in a gradient, with no internal breaks and tight connections. The molar percentage of nickel decreases from the center to the outer surface, while the molar percentage of manganese increases from the center to the outer surface. The innermost core is rich in nickel, which is beneficial to improving the discharge specific capacity of the sodium-ion battery cathode material, while the outermost layer is rich in manganese, which is beneficial to improving the cycle stability and structural stability of the sodium-ion battery cathode material.

[0041] In this invention, unless otherwise specified, preferably, "gradient increase" means that the molar percentage of manganese increases overall from the center of the sphere to the outer surface. As long as this overall upward trend is satisfied, the molar percentage of manganese at an outer point can be greater than or equal to the molar percentage of manganese at an inner point. "Gradient decrease" means that the molar percentage of nickel decreases overall from the center of the sphere to the outer surface. As long as this overall downward trend is satisfied, the molar percentage of nickel at an outer point can be less than or equal to the molar percentage of nickel at an inner point. More preferably, the contents of nickel and manganese in the sodium-ion battery precursor exhibit a linear gradient distribution along the radial direction; the nickel content decreases linearly from the center of the sphere to the outer surface, and the manganese content increases linearly from the center of the sphere to the outer surface.

[0042] In this invention, the distribution of nickel, manganese and M metal elements is tested using energy dispersive spectroscopy (EDS). The specific testing method includes: taking the center of the sodium-ion battery precursor as the midline for cross-sectioning, and taking sampling points every 0.5 μm from the center of the precursor to the outer surface for elemental composition testing.

[0043] In this invention, based on the total amount of nickel, manganese, and M metal in the innermost layer, the content of nickel in the innermost layer is 45-80 mol%, for example, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, and any value within any range of any two values, preferably 50-65 mol%; the content of manganese in the innermost layer is 0-30 mol%, for example, 0 mol%, 5 mol%, 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, and any value within any range of any two values, preferably 10-25 mol%.

[0044] In this invention, based on the total amount of nickel, manganese, and M metal in the outermost layer, the content of nickel in the outermost layer is 10-40 mol%, for example, 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, and any value within any range of any two values, preferably 20-35 mol%; the content of manganese in the outermost layer is 35-70 mol%, for example, 35 mol%, 40 mol%, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, and any value within any range of any two values, preferably 40-55 mol%.

[0045] In this invention, the particle size D of the precursor is... 50The value is 2-15 μm, for example, 1 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, and any value within the range of any two values, preferably 8-13 μm. In this invention, the D... 50 It refers to the particle size corresponding to a cumulative particle size distribution percentage of 50% for a sample.

[0046] In some embodiments of the present invention, preferably, the chemical formula of the sodium-ion battery precursor is Ni. x Mn y M z (OH), where 0.2≤x≤0.5, for example, can be 0.2, 0.3, 0.4, 0.5, or any value within the range of any two values; 0.2≤y≤0.8, for example, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or any value within the range of any two values; 0≤z≤0.5, for example, can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, or any value within the range of any two values; and x+y+z=1.

[0047] In this invention, M is selected from at least one of Fe, Mg, Al, Ti, W, Cu and Co, and preferably, M is Fe and / or Cu.

[0048] A second aspect of the present invention provides a method for preparing a sodium-ion battery precursor, wherein the method includes the following steps:

[0049] (1) Prepare nickel salt solution, manganese salt solution, M salt solution, precipitant solution and complexing agent solution respectively;

[0050] (2) Mix the precipitant solution, complexing agent solution and water to prepare the bottom liquid of the reaction vessel;

[0051] (3) Add nickel salt solution, manganese salt solution, M salt solution, precipitant solution and complexing agent solution to the bottom liquid of the reaction vessel at the same time and react to obtain a solid-liquid mixed slurry;

[0052] (4) The solid-liquid mixture is washed, dried and sieved to obtain the sodium-ion battery precursor;

[0053] Wherein, M is selected from at least one of Fe, Mg, Al, Ti, W, Cu and Co;

[0054] The flow rate of the added nickel salt solution is determined according to formula Q. Ni =S Ni +n Ni αt changes, where QNi S is the instantaneous flow rate of the nickel salt solution. Ni n is the initial flow rate of the nickel salt solution. Ni Let be the molar concentration of the nickel salt solution, α be the flow rate coefficient of the nickel salt solution, -0.02≤α≤-0.15, and t be the reaction time;

[0055] The flow rate of the added manganese salt solution is determined according to formula Q. Mn =S Mn +n Mn βt changes, where Q Mn S is the instantaneous flow rate of the manganese salt solution. Mn Let n be the initial flow rate of the manganese salt solution. Mn denoted as ωm, where ω is the molar concentration of the manganese salt solution, β is the flow rate variation coefficient of the manganese salt solution (0.02 ≤ β ≤ 0.15), and t is the reaction time.

[0056] In this invention, -0.02≤α≤-0.15 can, for example, be -0.02, -0.03, -0.05, -0.07, -0.09, -0.11, -0.13, -0.15, or any value within a range consisting of any two values; 0.02≤β≤0.15 can, for example, be 0.02, 0.03, 0.05, 0.07, 0.09, 0.11, 0.13, 0.15, or any value within a range consisting of any two values.

[0057] In this invention, the inventors discovered that by selecting different flow rate variation coefficients for nickel or manganese salt solutions based on different molar concentrations, the nickel and manganese content in the prepared sodium-ion battery precursor can be distributed in a radial gradient. This yields flow rate variation formulas for adding nickel and manganese salt solutions. Adding nickel and manganese salt solutions according to these flow rate variation formulas helps solve the problem of uneven concentration gradient distribution in sodium-ion battery cathode materials, thereby improving the cycle stability and structural stability of the sodium-ion precursor cathode material.

[0058] In this invention, the formula Q Ni =S Ni +n Ni αt and formula Q Mn =S Mn +n MnIn βt, t can be a time that changes continuously as the reaction proceeds, or a time that changes intermittently during the reaction. That is, the nickel and manganese contents in the obtained sodium-ion battery precursor are distributed in a radial gradient. In the preferred case, t is a time that changes continuously as the reaction proceeds, that is, the nickel content in the obtained sodium-ion battery precursor decreases linearly from the center of the sphere to the outer surface, and the manganese content increases linearly from the center of the sphere to the outer surface. The innermost layer is rich in nickel and the outermost layer is rich in manganese, which is beneficial to improving the discharge specific capacity, cycle stability and structural stability of the sodium-ion battery cathode material.

[0059] In some embodiments of the present invention, preferably, the nickel salt, manganese salt, and M salt are each independently selected from at least one of the sulfate, nitrate, chloride, acetate, and oxalate salts of nickel, manganese, and metal M.

[0060] In this invention, the precursor has the chemical formula Ni. x Mn y M z (OH)2, wherein 0.2≤x≤0.5, 0.2≤y≤0.8, 0≤z≤0.5, x+y+z=1, wherein M is selected from at least one of Fe, Mg, Al, Ti, W, Cu and Co, preferably, M is Fe and / or Cu.

[0061] In this invention, preferably, the nickel salt, manganese salt, and ferrous salt are prepared into an acidic salt solution, which is beneficial for inhibiting Fe. 2+ Oxidized to Fe 3+ The generation of small spheres can control the sodium-ion battery precursor to basically not produce small spheres during the growth process, and can successfully grow to the target particle size.

[0062] In this invention, the precipitant can be any precipitant known to those skilled in the art that can be used to prepare sodium ion electrode precursors and their cathode materials. Preferably, the precipitant is selected from at least one of sodium hydroxide, potassium hydroxide, and lithium hydroxide.

[0063] In this invention, the complexing agent can be any complexing agent known to those skilled in the art that can be used to prepare sodium ion electrode precursors and their positive electrode materials. Preferably, the complexing agent is selected from at least one of ammonia, ammonium sulfate, ammonium bicarbonate and oxalic acid, with ammonia being the most preferred.

[0064] In this invention, in order to better control the pH and NH4 in the reactor +To reduce fluctuations and viscosity of the liquid in the reactor, the salt solution, precipitant solution, and complexing agent solution were all diluted. Preferably, in step (1), the concentration of the nickel salt solution is 0.5-2.5 mol / L; the concentration of the manganese salt solution is 0.5-2.5 mol / L; the concentration of the M salt solution is 0.5-2.5 mol / L; the concentration of the precipitant solution is 3-10 mol / L; and the concentration of the complexing agent solution is 3-10 mol / L.

[0065] In some embodiments of the present invention, preferably, in step (2), the ammonia content of the bottom liquid of the reaction vessel is 2-15 g / L and the pH is 9-14.

[0066] In some embodiments of the present invention, preferably, the total volume of the precipitant solution, complexing agent solution and water is 40%-80% based on the volume of the reaction vessel.

[0067] In some embodiments of the present invention, preferably, in step (3), the reaction conditions include: the reaction is carried out under inert gas and stirring conditions, the reaction temperature is 40-70°C; the reaction time is 40-100h; the ammonia content of the reaction system is 2-15g / L; the pH of the reaction system is 8-13; and the stirring speed is 300-800rpm.

[0068] In this invention, the inert gas is beneficial for protecting Fe. 2+ To prevent it from being oxidized to Fe in the reaction system. 3+ This led to Ni 2+ Mn 2+ Precipitation occurs, resulting in the formation of small spheres. The inert gas described in this invention can be selected from at least one of nitrogen, helium, and argon. The flow rate of the inert gas is not particularly limited, but preferably, the flow rate is 4-6 L / min.

[0069] In this invention, preferably, step (3) includes: under stirring conditions, introducing an inert gas, heating to the reaction temperature, adding a nickel salt solution, a manganese salt solution, and a M salt solution using a precision flow pump and a precision mass flow meter, wherein the flow rates of the added nickel salt solution and manganese salt solution are according to the above flow rate change formula, and simultaneously pumping a precipitant solution and a complexing agent solution into the reaction system using a precision flow pump, controlling the ammonia content and pH of the reaction system by finely adjusting the flow rates of the complexing agent solution and the precipitant solution, and determining the particle size D of the product. 50 Once the target size is reached, the reaction is stopped, resulting in a solid-liquid mixture slurry. In this invention, the particle size D... 50 The particle size was measured using a Malvern particle size analyzer, with measurements taken every 1 hour.

[0070] In some embodiments of the present invention, preferably, the initial flow rate S of the nickel salt solution relative to a reaction vessel with a volume of 1 L is... Ni The value is 1 / 900-1 / 30 L / h. For example, it can be 1 / 900 L / h, 1 / 300 L / h, 1 / 150 L / h, 1 / 100 L / h, 1 / 75 L / h, 1 / 60 L / h, 1 / 50 L / h, 7 / 300 L / h, 4 / 150 L / h, 3 / 100 L / h, 1 / 30 L / h, or any value within the range of any two values, preferably 1 / 150-1 / 50 L / h.

[0071] In some embodiments of the present invention, preferably, the initial flow rate S of the manganese salt solution relative to a reaction vessel with a volume of 1 L is... Mn The value is 1 / 900-1 / 30 L / h. For example, it can be 1 / 900 L / h, 1 / 300 L / h, 1 / 150 L / h, 1 / 100 L / h, 1 / 75 L / h, 1 / 60 L / h, 1 / 50 L / h, 7 / 300 L / h, 4 / 150 L / h, 3 / 100 L / h, 1 / 30 L / h, or any value within the range of any two values, preferably 1 / 300-1 / 60 L / h.

[0072] In some embodiments of the present invention, preferably, the flow rate of the M salt solution relative to a 1L reactor is 1 / 900-1 / 30L / h, for example, it can be 1 / 900L / h, 1 / 300L / h, 1 / 150L / h, 1 / 100L / h, 1 / 75L / h, 1 / 60L / h, 1 / 50L / h, 7 / 300L / h, 4 / 150L / h, 3 / 100L / h, 1 / 30L / h, and any value within the range of any two values, preferably 1 / 150-1 / 60L / h.

[0073] In this invention, nickel salt, manganese salt, and M salt solutions are fed through a precision flow pump and a precision mass flow meter. The nickel salt solution and manganese salt solution are fed according to the above-mentioned flow rate change formula, which is beneficial to improve the precise control of the content of manganese, nickel, and M elements in the sodium-ion battery precursor. It is highly operable and has excellent processing performance.

[0074] In this invention, the washing method and conditions in step (4) are not particularly limited. For example, the washing solution may be selected from sodium hydroxide solution and / or sodium carbonate solution.

[0075] In this invention, the drying conditions are not particularly limited. For example, it can be carried out in a vacuum drying oven at 80-120°C for 8-12 hours.

[0076] In this invention, the sodium-ion battery precursor is spherical and / or near-spherical in shape. The precursor comprises nickel, manganese, and metal M, with the contents of nickel and manganese distributed in a radial gradient. M is selected from at least one of Fe, Mg, Al, Ti, W, Cu, and Co. The nickel content decreases gradient from the center to the outer surface, while the manganese content increases gradient from the center to the outer surface. Based on the total amount of nickel, manganese, and metal M in the innermost layer, the nickel content is 45-80 mol%, and the manganese content is 0-30 mol%. Based on the total amount of nickel, manganese, and metal M in the outermost layer, the nickel content is 10-40 mol%, and the manganese content is 35-70 mol%. The particle size D of the sodium-ion battery precursor is... 50 It is 2-15μm.

[0077] In this invention, the total amount of nickel, manganese, and M metal in each layer of the sodium-ion battery precursor is 100 mol%.

[0078] The third aspect of the present invention provides a sodium-ion battery cathode material, wherein the cathode material is obtained by gradient temperature sintering of a sodium-ion battery precursor prepared by the method described in the first aspect or the method described in the second aspect above with a sodium source.

[0079] In some embodiments of the present invention, preferably, the chemical formula of the positive electrode material is Na. m (Ni x Mn y M z O2, wherein 0.6≤m≤1.1, 0.2≤x≤0.5, 0.2≤y≤0.8, 0≤z≤0.5, x+y+z=1, and M is selected from at least one of Fe, Mg, Al, Ti, W, Cu and Co.

[0080] In some embodiments of the present invention, preferably, M is Fe and / or Cu.

[0081] In some embodiments of the present invention, preferably, the sodium source is selected from at least one of sodium hydroxide, sodium carbonate, sodium bicarbonate, sodium oxide, and sodium oxalate.

[0082] In this invention, the sodium-ion battery prepared from the sodium-ion battery cathode material exhibits an initial discharge specific capacity of 132-136 mAh / g at 0.1C rate; a discharge specific capacity of 119-125 mAh / g at 1C rate; and a capacity retention rate of 87-93% after 100 cycles at 0.2C rate. The sodium-ion battery cathode material has a gradient distribution structure, which helps to buffer the volume change of the core during charging and discharging, reduces structural collapse during repeated charging and discharging, improves the cycle stability and structural stability of the cathode material, and enhances the discharge specific capacity and cycle stability.

[0083] A fourth aspect of the present invention provides a method for preparing the sodium-ion battery cathode material described in the third aspect above, wherein the method includes:

[0084] The sodium-ion battery precursor and sodium source are mixed and then sintered at a gradient temperature to obtain the cathode material.

[0085] In some embodiments of the present invention, preferably, the molar ratio of the sodium-ion battery precursor to the sodium source is 1:1.01-1.25.

[0086] In some embodiments of the present invention, preferably, the gradient temperature sintering includes: a first sintering at a temperature of 300-600°C for 2-8 hours; and a second sintering at a temperature of 700-1100°C for 9-16 hours. In the present invention, the sintering atmosphere is not particularly limited; for example, sintering can be carried out in an air atmosphere.

[0087] In this invention, the method further includes grinding and sieving the product obtained by gradient heating sintering to obtain a sodium-ion battery cathode material. In this invention, the grinding and sieving method can be a conventional grinding and sieving method in the art.

[0088] In a preferred embodiment of the present invention, such as Figure 1 As shown, the method for preparing the sodium-ion battery precursor and its cathode material includes the following steps:

[0089] (1) Solution preparation: Prepare nickel salt, manganese salt and M salt solutions with concentrations of 0.5-2.5 mol / L respectively, and prepare precipitant solution and complexing agent solution with concentrations of 3-10 mol / L respectively;

[0090] (2) Preparation of reaction vessel bottom liquid: Add the precipitant solution, complexing agent solution and water to the reaction vessel, so that the total volume of the precipitant solution, complexing agent solution and water is 40%-80% of the volume of the reaction vessel, to obtain the reaction vessel bottom liquid;

[0091] (3) Introduce nitrogen into the sealed reactor, start stirring, and control the reaction temperature at 40-70℃. Add the nickel salt, manganese salt, M salt, sodium hydroxide solution and ammonia solution prepared in step (1) into the reactor. Control the ammonia content in the reaction system to be 2-15 g / L and the pH to be 8-13 by finely adjusting the flow rates of the precipitant solution and the complexing agent solution. As the metal salt solution continues to enter the reactor, the particle size in the system gradually increases. When the particle size D of the material in the reactor increases... 50 The reaction was stopped at 2-15 μm, and after the reaction was completed, a solid-liquid mixture was obtained.

[0092] (4) The obtained solid-liquid mixture slurry is washed, dried and sieved in sequence to obtain the sodium-ion battery precursor;

[0093] (5) The precursor is mixed with a sodium source, sintered by gradient heating, and then ground and sieved to obtain a sodium-ion battery cathode material.

[0094] The flow rate of the added nickel salt solution is determined according to formula Q. Ni =S Ni +n Ni αt changes, where Q Ni S is the instantaneous flow rate of the nickel salt solution. Ni n is the initial flow rate of the nickel salt solution. Ni Let be the molar concentration of the nickel salt solution, α be the flow rate coefficient of the nickel salt solution, -0.02≤α≤-0.15, and t be the reaction time;

[0095] The flow rate of the added manganese salt solution is determined according to formula Q. Mn =S Mn +n Mn βt change, where Q Mn S is the instantaneous flow rate of the manganese salt solution. Mn Let n be the initial flow rate of the manganese salt solution. Mn denoted as ωm, where ω is the molar concentration of the manganese salt solution, β is the flow rate variation coefficient of the manganese salt solution (0.02 ≤ β ≤ 0.15), and t is the reaction time.

[0096] The present invention will be described in detail below through embodiments.

[0097] In the following examples and comparative examples, the particle size D of the sodium-ion battery precursor is... 50 The testing methods for chemical composition are the same as those in the specific implementation method, and will not be repeated here.

[0098] The sodium-ion battery was tested for performance at 0.1C, 0.2C and 1C respectively, and the ratio of the discharge capacity after 100 cycles to the discharge capacity after the first cycle was used as the capacity retention rate.

[0099] Example 1

[0100] (1) Solution preparation: Prepare nickel sulfate, manganese sulfate and ferrous sulfate into 1.5 mol / L nickel salt solution, manganese salt solution and ferrous salt solution respectively, and prepare 6 mol / L sodium hydroxide solution and 8 mol / L ammonia solution for later use;

[0101] (2) Preparation of reaction vessel bottom solution: Add pure water, sodium hydroxide solution and ammonia solution to a 300L reaction vessel in sequence until the reaction vessel volume is 70%, adjust the ammonia concentration to 6g / L and the pH to 10.5 to prepare the reaction vessel bottom solution;

[0102] (3) Preparation of sodium-ion battery precursor: The temperature inside the reactor was controlled at 50℃, the stirring speed was 500 rpm, and nitrogen gas was introduced through the gas mass flow meter at a flow rate of 5 L / min. Nickel salt solution, manganese salt solution, and ferrous salt solution were pumped into the reactor at initial flow rates of 6 L / h, 1 L / h, and 3 L / h, respectively, using a precision metering pump and a precision mass flow meter. Sodium hydroxide solution and ammonia solution were pumped in simultaneously. The flow rate of the added nickel salt solution was determined according to formula Q. Ni =S Ni +n Ni αt changes linearly, and the flow rate of the added manganese salt solution is based on the formula Q. Mn =S Mn +n Mn βt changes linearly. At the end of the reaction, the flow rates of the nickel salt solution, manganese salt solution, and ferrous salt solution are 2 L / h, 5 L / h, and 3 L / h, respectively. The ammonia concentration in the reactor is controlled at 6 g / L, pH at 9.5, and the reaction time at 60 h by fine-tuning the flow rates of the sodium hydroxide solution and ammonia solution. The particle size D... 50 Once the particle size reaches 10 μm, the reaction is stopped, and a precursor slurry is obtained. The slurry is then washed, dried, and sieved to obtain a sodium-ion battery precursor.

[0103] (4) Weigh sodium carbonate according to a precursor to sodium carbonate molar ratio of 1:1.08, mix the precursor and sodium carbonate, heat from room temperature (25°C) to 500°C, keep warm for 3 hours, then gradually increase the temperature to 900°C, sinter for 15 hours, cool to room temperature, and obtain sodium-ion battery cathode material by grinding and sieving.

[0104] Figure 2The figure shows the elemental distribution of the sodium-ion battery precursor in this embodiment. As can be seen from the figure, the contents of nickel and manganese in the prepared sodium-ion battery precursor are distributed in a linear gradient along the radial direction, decreasing linearly from the center of the sphere to the outer surface, while the contents of manganese increase linearly from the center of the sphere to the outer surface. Specifically, the innermost layer contains 60 mol% nickel, 10 mol% manganese, and 30 mol% iron; the outermost layer contains 20 mol% nickel, 50 mol% manganese, and 30 mol% iron.

[0105] Example 2

[0106] (1) Solution preparation: Prepare nickel sulfate, manganese sulfate and ferrous sulfate into 1.5 mol / L nickel salt solution, manganese salt solution and ferrous salt solution respectively, and prepare 6 mol / L sodium hydroxide solution and 8 mol / L ammonia solution for later use;

[0107] (2) Preparation of reaction vessel bottom solution: Add pure water, sodium hydroxide solution and ammonia solution to a 300L reaction vessel in sequence until the reaction vessel volume is 70%, adjust the ammonia concentration to 6g / L and the pH to 10.5 to prepare the reaction vessel bottom solution;

[0108] (3) Preparation of sodium-ion battery precursor: The temperature inside the reactor was controlled at 50℃, the stirring speed was 500 rpm, and nitrogen gas was introduced through the gas mass flow meter at a flow rate of 5 L / min. Nickel salt solution, manganese salt solution, and iron salt solution were added to the reactor at initial flow rates of 5 L / h, 2 L / h, and 3 L / h, respectively, using a precision metering pump and a precision mass flow meter. Sodium hydroxide solution and ammonia solution were pumped in simultaneously. The flow rate of the added nickel salt solution was determined according to formula Q. Ni =S Ni +n Ni αt changes linearly, and the flow rate of the added manganese salt solution is based on the formula Q. Mn =S Mn +n Mn βt changed linearly. At the end of the reaction, the flow rates of the nickel salt solution, manganese salt solution, and iron salt solution were 3 L / h, 4 L / h, and 3 L / h, respectively. The ammonia concentration in the reactor was controlled at 6 g / L, the pH was 9.5, and the reaction time was 60 h by adjusting the flow rates of the sodium hydroxide solution and the ammonia solution. The particle size D 50 Once the particle size reaches 10 μm, the reaction is stopped, and a precursor slurry is obtained. The slurry is then washed, dried, and sieved to obtain a sodium-ion battery precursor.

[0109] (4) Sodium carbonate is weighed according to the precursor to sodium carbonate molar ratio of 1:1.06. The precursor and sodium carbonate are mixed and heated from room temperature (25°C) to 500°C, kept at that temperature for 3 hours, gradually increased to 900°C, sintered for 15 hours, cooled to room temperature, and then ground and sieved to obtain sodium-ion battery cathode material.

[0110] Figure 3 The figure shows the elemental distribution of the sodium-ion battery precursor in this embodiment. As can be seen from the figure, the contents of nickel and manganese in the prepared sodium-ion battery precursor are distributed in a linear gradient along the radial direction, decreasing linearly from the center of the sphere to the outer surface, while the contents of manganese increase linearly from the center of the sphere to the outer surface. Specifically, the contents of nickel in the innermost layer are 50 mol%, manganese in the innermost layer are 20 mol%, and iron in the innermost layer are 30 mol%; the contents of nickel in the outermost layer are 30 mol%, manganese in the outermost layer are 40 mol%, and iron in the outermost layer are 30 mol%.

[0111] Example 3

[0112] The method described in Example 1 is different,

[0113] In step (3), the initial flow rates of the nickel salt solution, manganese salt solution, and iron salt solution are 5.5 L / h, 1.5 L / h, and 3 L / h, respectively. The flow rate of the added nickel salt solution is determined according to formula Q. Ni =S Ni +n Ni αt changes linearly, and the flow rate of the added manganese salt solution is based on the formula Q. Mn =S Mn +n Mn The βt changes linearly, and at the end of the reaction, the flow rates of the nickel salt solution, manganese salt solution, and iron salt solution are 3 L / h, 4 L / h, and 3 L / h, respectively; thus, a sodium-ion battery precursor and a sodium-ion battery cathode material are obtained.

[0114] Figure 4 The figure shows the elemental distribution of the sodium-ion battery precursor in this embodiment. As can be seen from the figure, the contents of nickel and manganese in the prepared sodium-ion battery precursor are distributed in a linear gradient along the radial direction, decreasing linearly from the center of the sphere to the outer surface, while the contents of manganese increase linearly from the center of the sphere to the outer surface. Specifically, the contents of nickel in the innermost layer are 55 mol%, manganese in the innermost layer are 15 mol%, and iron in the innermost layer are 30 mol%; the contents of nickel in the outermost layer are 30 mol%, manganese in the outermost layer are 40 mol%, and iron in the outermost layer are 30 mol%.

[0115] Example 4

[0116] The method is the same as in Example 1, except that...

[0117] In step (2), pure water, sodium hydroxide solution and ammonia solution are added sequentially to the 300L reactor until the reactor volume is 70%, and the ammonia concentration is adjusted to 6g / L.

[0118] In step (3), the initial flow rates of the nickel salt solution, manganese salt solution, and iron salt solution are 7 L / h, 0 L / h, and 3 L / h, respectively; the flow rate of the added nickel salt solution is calculated according to formula Q. Ni =S Ni +n Ni αt changes linearly, and the flow rate of the added manganese salt solution is based on the formula Q. Mn =S Mn +n Mn The βt changes linearly. At the end of the reaction, the flow rates of the nickel salt solution, manganese salt solution, and iron salt solution are 1 L / h, 6 L / h, and 3 L / h, respectively. By adjusting the flow rates of the sodium hydroxide solution and the ammonia solution, the ammonia concentration in the reactor is controlled at 7 g / L, the pH is 10, and the reaction time is 80 h. The particle size D50 reaches 14 μm, and the reaction is stopped. Sodium-ion battery precursor and sodium-ion battery cathode material are obtained.

[0119] Example 5

[0120] The method is the same as in Example 1, except that...

[0121] In step (1), nickel sulfate, manganese sulfate and ferrous sulfate are prepared into 1 mol / L nickel salt solution, manganese salt solution and ferrous salt solution, respectively;

[0122] In step (2), pure water, sodium hydroxide solution and ammonia solution are added sequentially to the 300L reactor until the reactor volume is 60%, and the ammonia concentration is adjusted to 7g / L.

[0123] In step (3), the initial flow rates of the nickel salt solution, manganese salt solution, and iron salt solution are 7 L / h, 0 L / h, and 3 L / h, respectively. The flow rate of the added nickel salt solution is determined according to formula Q. Ni =S Ni +n Ni αt changes linearly, and the flow rate of the added manganese salt solution is based on the formula Q. Mn =S Mn +n Mn The βt changes linearly. At the end of the reaction, the flow rates of the nickel salt solution, manganese salt solution, and iron salt solution are 1 L / h, 6 L / h, and 3 L / h, respectively. By adjusting the flow rates of the sodium hydroxide solution and the ammonia solution, the ammonia concentration in the reactor is controlled at 7 g / L, the pH is 10, and the reaction time is 100 h. The particle size D50 reaches 14 μm, and the reaction is stopped. Sodium-ion battery precursor and sodium-ion battery cathode material are obtained.

[0124] Comparative Example 1

[0125] (1) Solution preparation: Dissolve nickel sulfate, manganese sulfate and ferrous sulfate in water at a molar ratio of 0.6:0.2:0.2 to prepare a 1 mol / L mixed salt solution A (200 L); dissolve nickel sulfate, manganese sulfate and ferrous sulfate in water at a molar ratio of 0.2:0.4:0.4 to prepare a 1 mol / L mixed salt solution B (400 L); prepare an 8 mol / L sodium hydroxide solution and an 8 mol / L ammonia solution for later use;

[0126] (2) Preparation of reaction vessel bottom solution: Add pure water, sodium hydroxide solution and ammonia solution to a 300L reaction vessel in sequence until the reaction vessel volume is 70%, adjust the ammonia concentration to 6g / L and the pH to 10.5 to prepare the reaction vessel bottom solution;

[0127] (3) Preparation of sodium-ion battery precursor: The temperature inside the reactor was controlled at 50℃, the stirring speed at 500 rpm, and nitrogen gas was introduced through the gas mass flow meter at a flow rate of 5 L / min. A mixed salt solution A was pumped into the reactor at a flow rate of 10 L / h using a precision metering pump and a precision mass flow meter. Simultaneously, a mixed salt solution B was pumped into mixed salt solution A at a flow rate of 6.667 L / h and mixed thoroughly. Sodium hydroxide solution and ammonia solution were also pumped in using a precision metering pump. The ammonia concentration in the reactor was controlled at 6 g / L and the pH at 9.5 by fine-tuning the flow rates of the sodium hydroxide solution and ammonia solution. The reaction time was 60 h. Both mixed salt solutions A and B were used up simultaneously. The particle size D... 50 Once the particle size reaches 10 μm, the reaction is stopped, and a precursor slurry is obtained. The slurry is then washed, dried, and sieved to obtain a sodium-ion battery precursor.

[0128] (4) Weigh sodium carbonate according to a precursor to sodium carbonate molar ratio of 1:1.08, mix the precursor and sodium carbonate, heat from room temperature (25°C) to 500°C, keep warm for 3 hours, then gradually increase the temperature to 900°C, sinter for 15 hours, cool to room temperature, and obtain sodium-ion battery cathode material by grinding and sieving.

[0129] Figure 5 The figure shows the elemental distribution of the sodium-ion battery precursor in this comparative example. As can be seen from the figure, the contents of nickel and manganese in the prepared sodium-ion battery precursor are distributed in a radial gradient. The nickel content decreases in a gradient from the center of the sphere to the outer surface, while the contents of manganese and iron increase in a gradient from the center of the sphere to the outer surface. The distribution curves of manganese and iron coincide. The innermost layer has a nickel content of 60 mol%, the innermost layer has a manganese content of 20 mol%, and the innermost layer has an iron content of 20 mol%. The outermost layer has the same contents of nickel, manganese, and iron, with a total of 100 mol%.

[0130] Comparative Example 2

[0131] (1) Solution preparation: Dissolve nickel sulfate, manganese sulfate and ferrous sulfate in water at a molar ratio of 1 / 3:1 / 3:1 / 3 to prepare a 1.5 mol / L mixed salt solution. Prepare an 8 mol / L sodium hydroxide solution and an 8 mol / L ammonia solution for later use.

[0132] (2) Preparation of reaction vessel bottom solution: Add pure water, sodium hydroxide solution and ammonia solution to a 300L reaction vessel in sequence until the reaction vessel volume is 70%, adjust the ammonia concentration to 6g / L and the pH to 10.5 to prepare the reaction vessel bottom solution;

[0133] (3) Preparation of sodium-ion battery precursor: The temperature inside the reactor was controlled at 50℃, the stirring speed at 500 rpm, and nitrogen gas was introduced through the gas mass flow meter at a flow rate of 5 L / min. The mixed salt solution was pumped into the reactor at a flow rate of 18 L / h using a precision metering pump. Sodium hydroxide solution and ammonia solution were pumped in simultaneously. The ammonia concentration in the reactor was controlled at 6 g / L and the pH at 10.5 by fine-tuning the flow rates of sodium hydroxide solution and ammonia solution. The reaction time was 60 h, and the internal particle size D was controlled at 6 g / L. 50 Once the particle size reaches 10 μm, the reaction is stopped, and a precursor slurry is obtained. The slurry is then washed, dried, and sieved to obtain a sodium-ion battery precursor.

[0134] (4) Sodium carbonate is weighed according to the precursor to sodium carbonate molar ratio of 1:1.08. The precursor and sodium carbonate are mixed, heated from room temperature (25°C) to 900°C, sintered for 15 hours, cooled to room temperature, and then ground and sieved to obtain sodium-ion battery cathode material.

[0135] Test case

[0136] The sodium-ion battery positive electrode materials prepared in Examples 1-5 and Comparative Examples 1-2 were assembled into button batteries. The button batteries were assembled using the sodium-ion battery positive electrode materials as the positive electrode material, Super P as the conductive agent, PVDF as the binder, NaPF6 as the electrolyte, a glass fiber membrane as the separator, and metallic sodium as the negative electrode material. The electrochemical performance of the button batteries was tested at 25°C and 2-4V. The test results are shown in Table 1.

[0137] Table 1

[0138]

[0139]

[0140] Combined with Examples 1-3, Figure 6As shown in Table 1, the sodium-ion battery precursor prepared by the method provided in this invention has a chemical composition that is uniformly distributed with a linear gradient. Its inner core is rich in nickel, and its outer layer is rich in manganese. The battery prepared by the sodium-ion cathode material provided in this invention has a high discharge specific capacity and excellent cycle retention rate. The initial discharge specific capacity at 0.1C rate is 132-136 mAh / g, the discharge specific capacity at 1C rate is 119-125 mAh / g, and the capacity retention rate after 100 cycles at 0.2C rate is 87-93%.

[0141] As can be seen from Examples 1, 4, and 5 and Table 1, the content of nickel and manganese in the innermost and outermost layers of the sodium-ion battery precursors in Examples 4 and 5 are not within the preferred range provided by this invention, and the particle size D of the sodium-ion battery precursors in Examples 4 and 5 is also not within the preferred range. 50 Outside the preferred scope provided by this invention, the discharge specific capacity and capacity retention rate of the battery prepared with sodium ion cathode material are slightly lower than those of Example 1.

[0142] In conjunction with Example 1 and Comparative Example 1, Figure 5 As can be seen from Table 1, Comparative Example 1, because it did not use the preparation method of the sodium-ion battery precursor provided by the present invention, prepared two mixed salt solutions with different molar ratios of nickel, manganese and ferrous salts. The elemental distribution of the prepared sodium-ion battery precursor showed a non-linear change, and the cycle retention rate of the prepared battery was low.

[0143] In conjunction with Example 1 and Comparative Example 2, Figure 6 As can be seen from Table 1, Comparative Example 2, due to the absence of the sodium-ion battery precursor preparation method provided by this invention and the adoption of the traditional co-precipitation method, resulted in a significant reduction in the battery's discharge specific capacity and cycle retention rate.

[0144] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A sodium-ion battery precursor, characterized in that, The sodium-ion battery precursor is spherical and / or near-spherical in shape, and comprises nickel, manganese, and metal M; M is Fe; the chemical formula of the precursor is Ni. x Mn y M z (OH)2, where 0.2 < x ≤ 0.5, 0.2 ≤ y ≤ 0.8, 0 < z ≤ 0.5, and x + y + z = 1; In the sodium-ion battery precursor, the contents of nickel and manganese are distributed in a linear gradient along the radial direction; the content of nickel decreases linearly from the center of the sphere to the outer surface, and the content of manganese increases linearly from the center of the sphere to the outer surface. Based on the total amount of nickel, manganese, and M metal in the innermost layer, the nickel content in the innermost layer is 50-65 mol%, and the manganese content in the innermost layer is 10-25 mol%. Based on the total amount of nickel, manganese, and M metal in the outermost layer, the nickel content in the outermost layer is 20-35 mol%, and the manganese content in the outermost layer is 40-55 mol%. Wherein, the particle size D of the sodium-ion battery precursor 50 It is 8-13μm.

2. A method for preparing the sodium-ion battery precursor of claim 1, characterized in that, The method includes the following steps: (1) Prepare nickel salt solution, manganese salt solution, M salt solution, precipitant solution and complexing agent solution respectively; (2) Mix the precipitant solution, complexing agent solution and water to prepare the bottom liquid of the reaction vessel; (3) Add nickel salt solution, manganese salt solution, M salt solution, precipitant solution and complexing agent solution to the bottom liquid of the reaction vessel at the same time and react to obtain a solid-liquid mixed slurry; (4) The solid-liquid mixture is washed, dried and sieved to obtain the sodium-ion battery precursor; Where M is Fe; The flow rate of the added nickel salt solution is determined according to formula Q. Ni =S Ni +n Ni αt changes, where Q Ni S is the instantaneous flow rate of the nickel salt solution. Ni n is the initial flow rate of the nickel salt solution. Ni Let be the molar concentration of the nickel salt solution, α be the flow rate coefficient of the nickel salt solution, -0.02≤α≤-0.15, and t be the reaction time; The flow rate of the added manganese salt solution is determined according to formula Q. Mn =S Mn +n Mn βt changes, where Q Mn S is the instantaneous flow rate of the manganese salt solution. Mn Let n be the initial flow rate of the manganese salt solution. Mn denoted as ωm, where ω is the molar concentration of the manganese salt solution, β is the flow rate variation coefficient of the manganese salt solution (0.02 ≤ β ≤ 0.15), and t is the reaction time.

3. The method according to claim 2, wherein, The nickel salt, manganese salt, and M salt are each independently selected from at least one of the sulfate, nitrate, chloride, acetate, and oxalate salts of nickel, manganese, and metallic M.

4. The method according to claim 2, wherein, The precipitant is selected from at least one of sodium hydroxide, potassium hydroxide, and lithium hydroxide.

5. The method according to claim 2, wherein, The complexing agent is selected from at least one of ammonia, ammonium sulfate, ammonium bicarbonate, and oxalic acid.

6. The method according to claim 5, wherein, The complexing agent is ammonia.

7. The method according to claim 2, wherein, In step (1), the concentration of the nickel salt solution is 0.5-2.5 mol / L; the concentration of the manganese salt solution is 0.5-2.5 mol / L; the concentration of the M salt solution is 0.5-2.5 mol / L; the concentration of the precipitant solution is 3-10 mol / L; and the concentration of the complexing agent solution is 3-10 mol / L.

8. The method according to claim 2, wherein, In step (2), the ammonia content of the bottom liquid of the reaction vessel is 2-15 g / L and the pH is 9-14.

9. The method according to claim 2, wherein, Based on the volume of the reactor, the total volume of the precipitant solution, complexing agent solution and water is 40%-80%.

10. The method according to claim 2, wherein, In step (3), the reaction conditions include: the reaction is carried out under inert gas and stirring conditions, the reaction temperature is 40-70℃, the reaction time is 40-100h, the ammonia content of the reaction system is 2-15g / L, the pH of the reaction system is 8-13, and the stirring speed is 300-800rpm.

11. The method according to claim 10, wherein, The inert gas is selected from at least one of nitrogen, helium, and argon.

12. The method according to claim 2, wherein, The initial flow rate S of the nickel salt solution relative to a 1L reactor. Ni It is 1 / 900-1 / 30 L / h.

13. The method according to claim 2, wherein, The initial flow rate S of the manganese salt solution relative to a 1L reactor. Mn It is 1 / 900-1 / 30 L / h.

14. The method according to claim 2, wherein, The flow rate of the M salt solution relative to a 1L reactor is 1 / 900-1 / 30L / h.

15. A sodium-ion battery cathode material, characterized in that, The cathode material is obtained by gradient temperature sintering of a sodium source with the sodium-ion battery precursor prepared by the method described in claim 1 or any one of claims 2-14.

16. The cathode material according to claim 15, wherein, The chemical formula of the positive electrode material is Na. m (Ni x Mn y M z O2, where 0.6≤m≤1.1, 0.2<x≤0.5, 0.2≤y≤0.8, 0<z≤0.5, x+y+z=1, and M is Fe.

17. The cathode material according to claim 16, wherein, The sodium source is selected from at least one of sodium hydroxide, sodium carbonate, sodium bicarbonate, sodium oxide, and sodium oxalate.

18. A method for preparing the sodium-ion battery cathode material according to any one of claims 15-17, wherein, The method includes: The sodium-ion battery precursor and sodium source are mixed and then subjected to gradient temperature sintering to obtain the cathode material.

19. The method according to claim 18, wherein, The molar ratio of the sodium-ion battery precursor to the sodium source is 1:1.01-1.

25.

20. The method according to claim 18, wherein, The gradient heating sintering includes: a first sintering at 300-600℃ for 2-8 hours; and a second sintering at 700-1100℃ for 9-16 hours.

Citation Information

Patent Citations

  • Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery

    CN108565457A

  • High-nickel-series and full-concentration gradient lithium ion battery positive electrode material and preparation method thereof

    CN105609759A

  • Composite positive electrode material, and preparation method and application thereof

    CN113851624A

  • Lithium secondary battery

    CN115548420A