Low dielectric, low thermal conductivity aerogel composites and methods of making the same

By using dispersion aqueous solution and atmospheric pressure drying technology in hydrolysis and condensation reactions, the problem of excessive use of organic solvents in the preparation of traditional aerogels is solved, realizing low-cost, high-purity, and low thermal conductivity aerogel composite materials, which are suitable for high-temperature environments and fields such as 5G and electric vehicles.

CN118026642BActive Publication Date: 2026-11-20TAIWAN AEROGEL TECH MATERIAL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202211415245.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-11
Publication Date
2026-11-20
Estimated Expiration
2042-11-11

AI Technical Summary

Technical Problem

Traditional aerogel preparation methods use large amounts of expensive and harmful organic solvents and surfactants, resulting in high costs, easy degradation of the product at high temperatures, impact on dielectric properties, difficulty in solvent recovery, and complex and cost-inefficient processes.

Method used

Hydrolysis and condensation reactions are carried out in a large amount of dispersed aqueous solution to avoid the addition of hydrophobic organic solvents and surfactants. The wet aerogel molecules are suspended and dispersed using an emulsifier and homogenizer. Combined with atmospheric pressure drying technology, alcohol solvents are recovered and rapidly dried at high temperature to form a low-cost, high-purity aerogel composite material with low thermal conductivity.

Benefits of technology

This technology enables low-cost production of aerogel composite materials with both low thermal conductivity and low dielectric properties, making them suitable for high-temperature environments. It simplifies the manufacturing process, reduces manufacturing costs and solvent recovery difficulties, and improves product purity and application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118026642B_ABST
    Figure CN118026642B_ABST
Patent Text Reader

Abstract

The application discloses a kind of low dielectric, low heat conduction aerogel composite material and its preparation method, in trace alcohol aqueous solution suspension dispersion to form trace alcohol aerogel suspension powder solution, can be uniformly compounded with various fiber blanket or fiber mat, then solvent recovery drying forms a low-cost, low-dielectric aerogel composite heat-insulating blanket, its steps include mixed hydrolysis, suspension dispersion condensation solution, composite forming and solvent recovery drying.This technology does not add a large amount of hydrophobic organic solvent and interfacial active agent, and in suspension dispersion condensation, a large amount of micro alcohol aqueous solution is combined with emulsifying machine to carry out direct suspension dispersion hydrophobic or hydrophilic-hydrophobic complex aerogel dispersion solution, then aerogel is compounded with various fiber blanket or mat using pressure suction, impregnation or spraying etc.Technology, with atmospheric pressure drying recovery technology carries out drying and solvent recovery reuse of aerogel composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a technique for preparing low-cost, low-dielectric, and low-thermal-conductivity hydrophobic or hydrophilic-hydrophobic complex aerogel composite materials. This technique avoids the addition of hydrophobic organic solvents and various additives during the hydrolysis and condensation steps of the preparation process. Instead, it directly suspends and disperses the aerogel condensation dispersion solution at high speed in an environment with a large amount of recovered hydrophilic solutions containing alcohol or other substances, forming an aerogel suspension dispersion colloidal solution. Compared to traditional aerogel melt-gel processes, this technique significantly reduces the use of large amounts of hydrophobic organic solvents (such as n-hexane, cyclohexane, benzene, toluene, xylene, etc.), acid-base catalysts for hydrolysis and condensation reactions, and the addition of surfactants, ammonia, and other additives. Therefore, this process can prepare low-cost, low-impurity hydrophobic or hydrophilic-hydrophobic complex aerogel insulating composite materials with low dielectric and low thermal conductivity. Background Technology

[0002] It is known that the thermal conductivity and dielectric properties of materials gradually decrease with increasing internal porosity. Therefore, aerogel materials and related composite materials can become energy-saving and carbon-reducing products with low thermal conductivity required by high-temperature manufacturing industries. They can also be used in 5G high-frequency signal transmission and electric vehicle lithium battery safety protection products. As is well known, aerogel is a porous material with a three-dimensional network structure. When its porosity is higher than 80% (even higher than 95%), aerogel materials have a low density (approximately 0.005 to 0.2 g / cm³). 3 High specific surface area (500 to 2,000 m²) 2Aerogels are technological products characterized by low thermal conductivity (k = 15 to 40 mW / mk), low dielectric properties (Dk = 1.3 to 2.5), and low dielectric loss (Df < 0.003). Due to these excellent properties, aerogels can be applied in industries such as high-temperature insulation, cold-weather insulation, sound insulation, and low-dielectric materials. Because the internal pore size of porous aerogels is only a few nanometers to tens of nanometers, aerogels have low thermal conductivity and heat convection properties. Therefore, regardless of whether it is an inorganic or organic aerogel, the higher the porosity in the material structure, the lower the thermal conductivity and dielectric properties. Therefore, in the future, industries such as petrochemical pipelines, metal smelting, building fireproofing and insulation, 5G low-dielectric materials, and high-frequency signal transmission in electric vehicles will require porous aerogels as the preferred product for industrial applications. However, current aerogel manufacturing processes require the use of large amounts of alcohols, ammonia, and hydrophobic solvents (such as n-hexane, cyclohexane, benzene, toluene, xylene, etc.) for mixing and solvent hydrophobic displacement, and the use of surfactants to prevent significant shrinkage and cracking during aerogel manufacturing. Therefore, while adding large amounts of organic solvents and surfactants to the process has its benefits, it significantly increases the overall manufacturing cost of aerogels and leads to defects in subsequent applications; for example, it can cause decomposition and odor at high temperatures, and the presence of large amounts of impurities and ions within the product will affect its dielectric properties.

[0003] The traditional method for preparing aerogels is the sol-gel synthesis technique. This involves mixing precursors such as alkoxysilanes, methyl orthosilicate, or water glass with an organic solvent, followed by the addition of an acid catalyst for hydrolysis. After a certain hydrolysis time, an alkaline catalyst is added to initiate a condensation reaction. During this condensation, a sol gradually forms, and the molecules within the sol continue to react and bond, gradually forming a semi-solid polymer gel. This gel is then aged for a period of time to form a stable three-dimensional network structure. Finally, solvent displacement is performed using solvents such as n-butanol, n-hexanol, n-hexane, or cyclohexane, followed by supercritical drying to extract and dry the solvent from the aerogel system. This process consumes large amounts of expensive and hazardous organic solvents and requires supercritical equipment. Furthermore, it necessitates lengthy solvent displacement using alcohols or alkanes, resulting in high-cost and time-consuming aerogels.

[0004] Therefore, current methods for preparing hydrophobic aerogels primarily involve mixing methyl alkyl silicate precursors such as methyltrimethoxysilane (MTMS) or methyltriethoxysilane (MTES) with an organic solvent, followed by the addition of an alkaline catalyst to initiate a hydrolysis reaction. After a certain period of hydrolysis, a condensation reaction occurs, gradually forming a sol. Within the sol, molecules continue to bond, gradually forming a semi-solid polymeric gel. After a period of aging, solvent replacement is performed for two to three days using organic solvents such as isopropanol, acetone, n-hexane, or cyclohexane, allowing the hydrophobic gel to form a stable three-dimensional network structure. Finally, the solvent in the aerogel system is dried using atmospheric pressure drying technology to obtain porous, dried aerogel blocks or composite materials. However, traditional aerogel preparation techniques require the use of large amounts of alcohols, such as ethanol, n-butanol, n-hexanol, and isopropanol, as well as large amounts of organic solvents, such as ammonia, cyclohexane, n-hexane, or toluene, for reactions or solvent displacement. Furthermore, the porosity of the aerogel increases with the content of the relevant alcohols and organic solvents. In addition, using supercritical or subcritical drying equipment for the drying of aerogel composites leads to drawbacks such as complex equipment procedures and high equipment costs.

[0005] The invention described in Chinese Invention Publication No. CN 113873697A and Taiwan Invention Publication No. I750717, entitled "Heat Insulation Component and Heating Assembly," provides a heat insulation component and a heating assembly. The heat insulation component includes a heat insulation material and a first covering heat insulation material, with the first covering layer sewn along a first seam to seal the heat insulation material. This heat insulation component prevents the dispersion of dust generated by the heat insulation material. A heating assembly incorporating the aforementioned heat insulation component is also provided. However, because aerogel dust particles are extremely small, using a covering layer made of silica gel, copper-based alkane lubricating oil, non-soap-based synthetic lubricating oil, lithium-based pressure-resistant grease, silicone-based grease, or molybdenum disulfide grease to coat the aerogel material, and then sewing the covering layer, while reducing aerogel dust dispersion, still cannot effectively and completely suppress the leakage of submicron and smaller aerogel dust, thus preventing indoor contamination of the cleanroom.

[0006] The "Flexible Composite Aerogel and Manufacturing Method" disclosed in Taiwan Invention Publication No. TW 201542457 mainly relates to a direct dispersion preparation method for a hydrophilic aerogel. The method pertains to a flexible composite organic aerogel comprising: a textile reinforcing material, wherein an organic aerogel is placed within the textile reinforcing material. The organic aerogel is based on a resin at least partially derived from polyhydroxybenzene and formaldehyde; the organic aerogel is a polymeric organic gel containing at least one water-soluble cationic polyelectrolyte; or the organic aerogel is a thermal decomposition product of the gel in the form of porous carbon monoliths, containing the thermal decomposition product of the at least one water-soluble cationic polyelectrolyte.

[0007] The invention disclosed in Taiwan Patent Publication No. TW I655094, entitled "Aerogel Composite and Method for Preparing the Aerogel Composite," primarily relates to an aerogel composite. This aerogel composite comprises at least one base layer having an upper surface and a lower surface, the base layer containing a reinforcing aerogel composition comprising a reinforcing material and a monolithic aerogel framework; a first facing layer comprising a first facing material adhered to the upper surface of the base layer; and a second facing layer comprising a second facing material adhered to the lower surface of the base layer. At least a portion of the monolithic aerogel framework of the base layer extends into a portion of both the first and second facing layers. The first and second facing materials may each comprise elastic fibers such as spandex, nylon, Lycra, elastic fibers, or combinations thereof, or may be primarily composed of elastic fibers. However, since the prepared aerogel coating material contains elastic fibers or soft polymer films, and the adhesive materials used are organic adhesives such as acrylate, ethyl carbamate, and hot melt adhesives, although the related soft products have good protective properties for the aerogel.

[0008] The invention disclosed in Taiwan Patent Publication No. TW I663062, entitled "Aerogel Composite and Preparation Method Thereof," relates to a method for preparing a gel-fiber composite by wetting a fibrous material comprising at least one of inorganic and organic fibers; laminating the wetted fibrous material and the spacer in a wound structure or in a planar form; filling the fibrous material into a container; preparing a gel-fiber composite by injecting a precursor into the container and gelling the precursor while removing residual air bubbles under vacuum; removing the aerogel-fiber composite from the container and removing the spacer; modifying the gel-fiber composite with solvent substitution and organic surface, and then drying the organically modified gel-fiber composite with atmospheric pressure or supercritical drying.

[0009] The "Laminated Body Containing Reinforced Aerogel Composite Material" described in Taiwan Invention Publication No. TW I743082 relates to an aerogel composite material. This aerogel composite material includes at least one base layer having a top surface and a bottom surface. The base layer includes a reinforcing aerogel composition and a monolithic reinforced aerogel framework. The composition includes a reinforcing material, a first face layer comprising a first face material attached to the top surface of the base layer, and a second face layer comprising a second face material attached to the bottom surface of the base layer. At least a portion of the monolithic aerogel framework of the base layer extends into at least a portion of both the first and second face layers. The first and second face materials are substantially each composed of a fluoropolymer material.

[0010] The invention disclosed in Taiwan, China, under patent number TW I765609, describes a method for manufacturing aerogel felt. This method involves first injecting aerogel slurry into a glass fiber felt, and then using an impregnation solution to form a sealing coating on the surface of the glass fiber felt. This prevents the aerogel felt from shedding powder during storage, transportation, and use. Therefore, it ensures that the amount of aerogel in the aerogel felt does not decrease, thus not affecting the thermal insulation performance of the aerogel felt. The surface sealing coating is a mixture of acrylic emulsion, talc, VAE emulsion, and a water-based curing agent.

[0011] The "Non-woven / Aerogel Composite Fireproof / Heat Insulation Material and its Preparation Method" described in Taiwan Invention Publication No. TW I535658 by our team involves preparing an aerogel through a hydrolysis step and a condensation step. Then, during the molding step, the aforementioned aerogel is added to a non-woven fabric, allowing the aerogel to fully penetrate the non-woven fabric. After a drying process, a non-woven / aerogel composite fireproof / heat insulation material is formed. The aerogel is fully penetrated into the non-woven fabric through an impregnation process or a continuous rolling process. The drying process is carried out under the conditions of anhydrous aerogel drying at room temperature and pressure, or by rapid vaporization drying of an organic solution between 30 and 80 degrees Celsius.

[0012] US Patent Publication No. 8,945,677B2, entitled "Manufacturing Electronic Devices Using Low-K Dielectric Materials," primarily describes materials and methods for manufacturing electronic devices and semiconductor components using low-dielectric materials (including polyimide aerogel). This prior art patent further provides methods for manipulating the properties of dielectric materials and influencing the overall dielectric properties of a system. Specifically, a sol-gel mixture is formed by mixing a polyurethane presol, a catalyst, and a polar solvent. The sol components are then crosslinked to form a wet gel material, and the solvent is removed using supercritical fluid to form a polyimide aerogel film. This technology is then used to combine the polyimide aerogel film with a non-porous, low-k template substrate. The prior art uses low-k dielectric materials to manufacture electronic devices and employs a multi-stage supercritical fluid process for solvent removal via pressure cycling. This overall technology is time-consuming and costly, and the process time is too long, making it uneconomical.

[0013] Chinese invention patent publication CN102044525A, entitled "Low-K Dielectric Layer Structure, Semiconductor Device Structure and Formation Method Thereof," primarily uses silica aerogel to form a low-k dielectric layer structure. This prior art patent also provides a semiconductor device structure and its formation method, wherein the formation method includes: providing a substrate, on which a first dielectric layer and an etch barrier layer are formed, both the first dielectric layer and the etch barrier layer having openings, the openings being filled with metal as plugs; forming a sacrificial oxide layer on the etch barrier layer and the plugs; forming an opening in the sacrificial oxide layer, filling the opening with metal to form an interconnect structure, wherein this interconnect structure is electrically connected to the plugs; selectively removing the sacrificial oxide layer to form gaps between the interconnect structures; and forming silica aerogel as a low-k dielectric layer in the gaps between the interconnect structures. This prior art patent uses a low-k dielectric layer structure and utilizes tetraethyl orthosilicate (TEOS) or tetramethyl orthosilicate (TMOS) as the material structure. In addition, the drying process involves multiple steps of low-dielectric thin film preparation using room temperature or supercritical fluid technology, which is time-consuming and costly. The process takes too long and is not cost-effective.

[0014] Chinese invention patent publication CN105189104A, entitled "Aerogel Insulating Panel and Manufacturing Thereof," primarily uses polyimide aerogel to prepare an insulating panel, which can be applied to laminated panels for aerospace applications. This panel includes a polyimide aerogel surface layer and a reflective protective layer on the surface layer. The process for manufacturing the polyimide aerogel in this prior art patent includes: (a) polymerizing a mixture of dianhydride and diamine monomers in a bipolar alkaline solvent (DMAc or NMP) to form a polyamic acid solution; (b) casting the polyamic acid solution into fiber filaments; (c) gelling the polyamic acid solution using acetic anhydride and pyridine via a chemical imidization reaction; and (d) removing the solvent from the gel using supercritical or subsupercritical CO2 drying technology to form a fiber / polyimide aerogel composite material.

[0015] US Patent Publication No. 9,777,126B2, entitled "Aerogel / Polymer Composite Material," comprises an aerogel and a thermoplastic polymer material, wherein the weight ratio of the aerogel to the thermoplastic polymer is less than 20:100. This composite material exhibits excellent insulation properties, good flexibility at low temperatures, and low brittleness.

[0016] The Chinese invention patent publication number CN108203516A, "Method for preparing cross-linked polyimide aerogel," mainly employs the sol-gel method, which includes: (a) polymerizing a mixture of dianhydride and diamine monomers in a bipolar alkaline solvent (DMAc or NMP) to form a polyamic acid solution; (b) casting the polyamic acid solution into fiber flocs; (c) using a chemical imidization reaction to gel the polyamic acid solution with acetic anhydride and pyridine; and (d) using supercritical or subsupercritical CO2 drying technology to remove the solvent from the gel to form a fiber / polyimide aerogel composite material.

[0017] Our team's invention, as described in Taiwan Patent Publication No. TW I643888, is a "Preparation Method of Aerogel / Composite Nonwoven Fireproof and Thermal Insulation Material." This method involves a mixing step, a hydrolysis step, and a condensation step to form a condensation solution of an ungelled silica-silicone aerogel-silane coupling agent aerogel solution. Then, in a molding step, this ungelled silica-silicone aerogel-silane coupling agent aerogel solution is impregnated, sprayed, sprayed, or subjected to continuous pressure suction of the solution onto a recycled composite nonwoven blanket or a general nonwoven blanket. This causes the silica-silicone aerogel-silane coupling agent aerogel to gel and interweave within the nonwoven blanket. A drying process is then performed to form an aerogel / composite nonwoven fireproof and thermal insulation material. The drying process is performed at room temperature and pressure for aerogel drying, or using a rapid vaporization drying process of an organic solution between 30 and 80 degrees Celsius. The nonwoven material is made of polyethylene (PE), polypropylene (PP), polyester, polyamide, or glass fiber. A relatively dust-free aerogel composite material made from one or a combination of fiber, rock wool, or other materials.

[0018] Traditional sol-gel techniques for manufacturing porous aerogels require the addition of large amounts of organic solvents during the hydrolysis and condensation reactions of the sol-gel reaction. These solvents include large quantities of alcohol, water, hydrophobic n-hexane or cyclohexane, and even toluene or benzene, to reduce shrinkage or cracking of aerogel molecules during drying. Furthermore, acid and base ions are added as catalysts during hydrolysis and condensation, and, as in the technology disclosed in Taiwan Patent Publication No. I705096, large amounts of surfactants or other additives are used. Therefore, prolonged solvent replacement or extensive cleaning with deionized water is necessary in the later stages of the process to produce suitable aerogel products or to maintain the stability of the aerogel structure during drying. Alternatively, using supercritical or subsupercritical CO2 drying technology to remove solvents from the gel can effectively produce high-quality aerogel materials, but each of these techniques has its advantages and disadvantages.

[0019] The biggest drawback of the above process is the use of large quantities of expensive and environmentally and safety-hazardous organic solvents, such as hydrophobic hexane, cyclohexane, toluene, or benzene, as well as large amounts of alcohols and ammonia. Aerogel preparation also involves multiple stages of solvent replacement at room temperature and pressure. This solvent replacement process uses large quantities of isopropanol, n-butanol, n-hexane, cyclohexane, toluene, or polyhalogenated benzenes. These techniques are all employed during the drying process to reduce the interfacial tension of water molecules within the aerogel, inducing significant shrinkage and cracking. Furthermore, this solvent replacement process takes more than 48 to 72 hours. This excessive time significantly increases the cost of aerogel preparation. The recovery and purification of the various organic solvents used in the process is also difficult. The process is complex, highly dangerous, and time-consuming, making it uneconomical.

[0020] Among the drawbacks of the aforementioned thermal insulation or low-dielectric electrogel patents, the main disadvantage lies in the use of large amounts of hydrophobic organic solvents and surfactants in aerogel manufacturing. Additionally, the bonding technology between aerogels and fiber materials primarily employs direct preparation methods, such as soaking in different aerogel slurries, bonding with organic adhesives, or the soft silicone blending method used in our previous technology. When these traditional aerogel composites are applied in high-temperature environments, the related organic adhesives undergo thermal decomposition. After decomposition, aerogel powder begins to fall from the interior of the composite material, leading to a rapid decline in its high-temperature insulation performance. Especially under prolonged temperatures above 250 degrees Celsius, the organic aerogels (polyimide aerogels), organic modifiers, or organic adhesives used in the aforementioned patents gradually decompose at 250 degrees Celsius, generating large amounts of toxic gases. This is another significant drawback of aerogel composites in high-temperature applications.

[0021] In view of the shortcomings of the prior art, the inventor conceived of an improvement idea and immediately conducted in-depth research and development. After a long period of effort in product improvement and technology development, this invention was finally born. The main objective of this invention is to provide a method for manufacturing an aerogel composite material that combines low cost, high purity (low dielectric constant), and low thermal conductivity. Summary of the Invention

[0022] One objective of this invention is to improve the shortcomings of the production technology of the above-mentioned hydrophobic or hydrophilic-hydrophobic complex aerogel composite materials. For example, traditional hydrophobic aerogel blankets require the addition of a large amount of hydrophobic organic solvents, which increases the manufacturing cost due to the large amount of organic solvents. Therefore, effectively reducing the amount of organic solvents, surfactants, and organic adhesives added in the process can significantly reduce the manufacturing cost, reduce the process risk, and improve the purity of the product to increase its applicability.

[0023] Another objective of this invention is to improve upon the shortcomings of organic solvent recovery in the manufacturing of related hydrophobic or hydrophilic-hydrophobic complex aerogel composite materials. For example, traditional hydrophobic aerogel processes utilize mixtures of various solvents. Recovering, distilling, and purifying these organic solvent mixtures for reuse requires significant energy and equipment costs. Furthermore, the distillation separation of multiple organic solvents often involves azeotropes, making it difficult to effectively purify organic solvents and reduce costs associated with their use in the process. In this technology, alcohols produced during hydrolysis or condensation reactions, primarily methanol and ethanol, are utilized as recovered alcohols. These recovered alcohol aqueous solutions, along with the recovered distilled water, can all be recycled and reused. Since these recovered alcohol aqueous solutions do not contain other hydrophobic solvents during purification, the recovery technology is simpler, significantly reducing the investment in solvent recovery equipment and costs.

[0024] Another objective of this invention is to overcome the shortcomings of the aforementioned hydrophobic or hydrophilic-hydrophobic complex aerogel composite products. For example, traditional hydrophobic aerogel materials, due to the addition of surfactants or emulsifiers during preparation, accumulate large amounts of surfactants or emulsifiers within the aerogel composite, significantly affecting its hydrophobic, thermal insulation, and dielectric properties. Furthermore, these products experience severe organic matter thermal decomposition at high temperatures (approximately 200 degrees Celsius), producing large amounts of toxic substances and odors, thus significantly limiting the application temperature range of the developed products.

[0025] Another objective of this invention is to develop an improved sol-gel synthesis technique combined with suspension dispersion technology to prepare hydrophobic or hydrophilic-hydrophobic complex aerogel composite materials without the need for adding large amounts of dispersing organic solvents and surfactants. Therefore, by using an emulsifier or homogenizer to suspend and disperse hydrophobic aerogel wet molecules in a large amount of aqueous solution, the particle size and porosity of the hydrophobic or hydrophilic-hydrophobic complex aerogels can be easily controlled, thereby enabling continuous or batch mass production of hydrophobic or hydrophilic-hydrophobic complex aerogel composite materials that combine low cost, high purity, and low thermal conductivity.

[0026] Another objective of this invention is to improve the long solvent replacement process in the traditional hydrophobic aerogel composite material manufacturing process, and to mass-produce aerogel composite materials with low cost, high purity and low thermal conductivity without using expensive supercritical drying technology.

[0027] Therefore, to overcome the drawbacks of past aerogel composite product preparation processes, such as the use of large amounts of organic solvents and the susceptibility to high-temperature organic degradation during application, this technology first involves condensing and dispersing the hydrolyzed solution in a large amount of dispersed water during the aerogel composite product preparation process. This solution is then composited onto a pre-formed fiber blanket or any substrate, followed by gelation molding. Subsequently, an alcohol-containing aqueous solution is vaporized and dried in a normal pressure and high-temperature environment. During vaporization and drying, the recoverable alcohol-containing azeotropic solution is recycled and reused, or the related alcohols are collected as byproducts. Further, trace amounts of solvent in the product are rapidly dried and vaporized at even higher temperatures. This approach allows for the preparation of low-cost, high-purity aerogel composite materials with low thermal conductivity, while also enabling the recovery of valuable byproducts. The hydrophobic aerogel / inorganic fiber products developed using this technology can be applied to energy-saving, carbon-reducing, and energy-efficient aerogel composite materials required for insulation in high-temperature pipelines (above 800 degrees Celsius), high-temperature boilers, and smelting boilers. They can also be applied in industries such as 5G low-dielectric applications, high-frequency signal transmission in electric vehicles, and lithium battery safety protection.

[0028] A low dielectric and low thermal conductivity aerogel composite material and its preparation method, wherein the embodiment of the present invention includes: (1) a mixing and hydrolysis step: adding a siloxane precursor to an aqueous solution containing trace amounts of alcohol and stirring to form a mixed solution, wherein the siloxane precursor includes siloxane compounds (such as TEOS, TEMS) and hydrophobically modified siloxane compounds (MTMS, MTES) or a combination thereof, and then adding an acid catalyst solution to the mixed solution to carry out a hydrolysis reaction; (2) a suspension dispersion condensation solution step: adding a large amount of an aqueous solution containing trace amounts of alcohol to the hydrolysis solution and using a dispersion device such as an emulsifier and homogenizer for rapid dispersion, so that the hydrolysis solution is dispersed in the aqueous solution to carry out a condensation reaction, wherein the suspension dispersion condensation suspension includes an alkaline catalyst to catalyze the condensation reaction to accelerate the formation and gradual gelation in the suspension dispersion solution; (3) a composite Synthesis step: The suspension dispersion condensation solution is rapidly injected into the fiber substrate by pressure suction, impregnation or spraying technology, and the suspension dispersion sol solution is further condensed inside the fiber substrate to form a three-dimensional network structure of aerogel wet glue fiber composite structure; (4) Solvent recovery and drying step: Under normal pressure, the solvent inside the aerogel wet glue fiber composite structure is vaporized at the molding drying temperature, and the vaporized vapor is condensed and recovered through heat exchange equipment, and the aerogel / fiber composite material is expanded during the drying period to obtain aerogel / fiber composite material with uniform structure and low thermal conductivity and low dielectric properties; Among them, the above process technology can obtain low cost, high purity and low thermal conductivity aerogel composite material, and the combined product will have industrial applications with low thermal conductivity and low dielectric properties.

[0029] Furthermore, in the above preparation method, the siloxane compound comprises tetramethoxysilane (TMOS), tetraethoxysilane (TEOS), or a combination thereof; the hydrophobically modified siloxane compound comprises methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), or a combination thereof, wherein, in the overall mixture, the molar ratio of the siloxane compound to the hydrophobically modified siloxane compound is between 0:100 mol% and 45:55 mol%. The purpose of adding the hydrophobically modified siloxane compound is to reduce the cracking phenomenon of the aerogel structure during the drying process; on the other hand, the purpose of adding the siloxane compound is to provide regulation of the internal microstructure of the aerogel structure and increase the pore structure and porosity in the structure, so as to reduce thermal conductivity or improve thermal insulation properties.

[0030] Furthermore, in the mixed hydrolysis step (1), the higher the content ratio of the acid catalyst in the mixed solution, the faster the hydrolysis rate. However, a large number of acid ions will generate ionic conductivity under the action of an electric field, which will significantly increase the dielectric constant and dielectric loss of the aerogel structure. In contrast, the lower the content ratio of the acid catalyst, the slower the overall hydrolysis rate. Therefore, this invention increases the hydrolysis rate of trace acid ions by reducing the acid catalyst content and increasing the process temperature, which can significantly reduce the overall content of added acid radical ions. On the other hand, siloxane compounds and hydrophobic siloxane compounds will generate a large number of alcohol molecules (such as methanol and ethanol) during the hydrolysis process. Therefore, deionized water is used to replace organic solvents such as ammonia and alkanes during the hydrolysis process, thereby reducing the addition of organic solvents such as ammonia and alkanes. In addition to reducing the influence of organic solvents such as ammonia on the dielectric properties of aerogel, it can also reduce the harmfulness of organic solvent treatment in the process and reduce the overall preparation cost of aerogel.

[0031] Furthermore, in the above preparation method, the aqueous solution containing trace amounts of alcohols in the mixed solution includes newly added methanol, ethanol and isopropanol, recovered methanol, ethanol and isopropanol, process recovery water, deionized water, distilled water, double-distilled water or a combination thereof.

[0032] Furthermore, in the (2) suspension dispersion condensation solution step, under the impetus of the alkaline catalyst aqueous solution and a large amount of dispersion solution, the siloxane molecules or hydrophobic siloxane molecules of the hydrolyzed solution will form a suspension dispersion condensation solution of nano- to sub-micron-sized molecules under the rapid stirring of the emulsifier or homogenizer.

[0033] Furthermore, in the above-mentioned (2) suspension dispersion condensation solution step, the preparation method of the low thermal transfer aerogel material provided by the present invention only adds a large amount of process recycled water, deionized water, distilled water, double distilled water or a combination thereof, including a small amount of newly added alcohols such as methanol, ethanol and isopropanol, and recycled alcohols such as methanol, ethanol and isopropanol. No large amount of hydrophobic organic solvents such as toluene, benzene, cyclohexane, etc., and no surfactants or other additives are added. Only hydrolyzed siloxane molecules or hydrophobic siloxane molecules are rapidly stirred in an emulsifier or homogenizer, causing the hydrolyzed siloxane molecules or hydrophobic siloxane molecules to form a suspension dispersion condensation solution of nano- to sub-micron-sized molecules. This reduces the particle size of the siloxane molecules or hydrophobic siloxane molecules, rapidly increasing the specific surface area of ​​the product. Therefore, the drying rate can be rapidly increased during drying, thus eliminating the need for subsequent multiple replacements of hydrophobic organic solvents to reduce the interfacial tension of water molecules, thereby preparing a high-purity, low thermal transfer aerogel composite material.

[0034] Furthermore, in the composite molding step (3): the suspended dispersion condensation solution is rapidly absorbed into the substrate such as fiber blankets and fiber mats using techniques such as pressure suction, impregnation, and spraying. This causes the hydrolyzed siloxane compounds and hydrophobic siloxane molecules to condense and aggregate in the substrate to form nano- to submicron-sized aerogel wet aggregates. Subsequently, these aggregates in the substrate to form a three-dimensional network gel structure. In this wet gel fiber blanket structure, the solvent content of the trace alcohol hydrolysis solution is the pore content within the aerogel particle structure; in addition, the content of the large amount of dispersed trace alcohol aqueous solution added in the condensation reaction is the pore content outside the aerogel network structure in the aerogel composite material. Therefore, in this technology, the trace alcohol aqueous solution without hydrophobic organic solvent added in the hydrolysis and condensation reactions can be used to control the aerogel pore structure inside the aerogel composite material and the pore content between the aerogel aggregate structures. In another embodiment, the suspended dispersion condensation solution can also be directly applied using pressure impregnation technology combined with continuous fiber mat or fiber blanket roll-up spraying process technology. This allows the nano- to submicron-sized hydrolyzed siloxane molecules and hydrophobic siloxane molecules in the suspended dispersion condensation solution to be uniformly dispersed inside the fiber blanket during the continuous roll-up process. The gelation time of the suspended dispersion condensation solution is controlled by the acid-base concentration ratio, enabling the suspended dispersion condensation solution to bond with the fiber substrate within a very short process time and form a stable wet aerogel / fiber blanket structure. Subsequently, the wet aerogel / fiber blanket is further rolled up and dried using infrared, ultraviolet, high-temperature roller, or other drying equipment.

[0035] Furthermore, in the above preparation method, the substrate such as the fiber blanket or fiber mat includes one or a combination of various inorganic fibers, various liquid crystal fibers, and various organic fibers in the form of blankets, cloths, or mats. Specifically, it includes one or more combinations of glass fibers, carbon fibers, quartz fibers, ceramic fibers, rock wool fibers, Kevlar polyamide fibers, Nomex polyamide fibers, polyimide fibers such as PI or PEI, Nylon fibers, PET polyester fibers, PE polyethylene fibers, PP polypropylene fibers, cellulose fibers, and modified cellulose fibers in the form of blankets, cloths, or mats.

[0036] Furthermore, in the above (3) composite molding step, bottom (top) vacuum technology can be combined to carry out composite molding such as impregnation, pressure suction, spraying, and atomization. The hydrolyzed siloxane molecules and hydrophobic siloxane molecules suspension dispersion condensation solution can be injected into the fiber-containing substrate at a faster speed for composite processing.

[0037] Furthermore, the solvent drying and recovery step (4) includes: a solvent vaporization drying step and a solvent recovery step: in the solvent vaporization drying step, the solid aerogel / fiber composite blanket molding structure is placed in an environment of atmospheric pressure and azeotropic temperature of mixed solvent, so that a large amount of mixed solvent in the solid aerogel / fiber composite molding structure is rapidly azeotropically vaporized and the solvent is vaporized and dried. The vaporization temperature is generally between 60 and 110°C; and a boiling step: the drying temperature of the dried aerogel / fiber composite blanket molding structure is adjusted to above the boiling temperature of the aqueous solution, so that the remaining water inside the nearly dried aerogel blanket generates a rapid boiling and forms a positive pressure. The positive pressure between the three-dimensional structures of the aerogel is used to suppress the shrinkage behavior of the aerogel during the drying process. In addition, the positive pressure inside the aerogel structure can also be used to promote the expansion of the aerogel structure and generate a large number of nano- to sub-micron-sized micropores to improve the porosity and thermal insulation properties of the aerogel product. The boiling temperature is between 110 and 180°C.

[0038] Furthermore, in the drying step (4) above, after the solid aerogel / fiber composite structure is stabilized, the alcohol-containing aqueous solution inside the wet aerogel structure is evaporated under normal pressure and at the molding drying temperature. In some embodiments of the present invention, the molding drying step (4) further includes a solvent vaporization step (4-1) and a boiling step (4-2). In the solvent vaporization step (4-1), the alcohol-aqueous solution contained in the solid aerogel / fiber composite structure is rapidly vaporized at an azeotropic temperature for drying. In the boiling step (4-2), the temperature of the aerogel close to the drying temperature is adjusted to the boiling temperature, so that the trace amount of alcohol-aqueous solution contained inside the aerogel undergoes rapid boiling. At this boiling temperature, the alcohol-aqueous solution contained in the aerogel structure generates positive pressure inside the aerogel. This positive pressure can suppress the shrinkage or collapse of the aerogel structure during the drying process.

[0039] Furthermore, in the solvent drying and recovery step (4) above, after the solid aerogel wet gel structure is stabilized, under normal pressure and at the azeotropic temperature of the mixed solvent at the molding drying temperature, a large amount of alcohol-containing aqueous solution in the molded structure is rapidly azeotropically vaporized, and the relevant vaporized vapor is guided to a plate heat exchanger; in the plate heat exchanger, the alcohol-containing aqueous solution is condensed and recovered; in some embodiments of the present invention, the condensed alcohol-containing aqueous solution is an additional recovery product of this process. The purpose of this recovery is, on the one hand, to recover valuable alcohol by-products to reduce manufacturing costs; on the other hand, to recover alcohol vapors to reduce pollution to the environment and air.

[0040] The preparation method provided by this invention has the following advantages:

[0041] 1. The preparation technology of the present invention is to modify the traditional sol-gel reaction process to prepare a strongly hydrophobic aerogel composite material or a composite aerogel composite material. Since no large amount of hydrophobic organic solvents, surfactants and other substances are added in the acid hydrolysis and alkali condensation reaction, the manufacturing cost can be significantly reduced. In addition, there is no need to use long-term solvent replacement or water washing or rinsing with deionized water in the subsequent process. Therefore, the overall process is simple, low-cost and highly efficient. Thus, this process has obvious economic competitive advantages.

[0042] 2. The preparation technique of this invention utilizes different proportions of siloxane compounds and methylsiloxane compounds to prepare composite aerogel materials with high or varying hydrophobicity. Furthermore, the differences in hydrophilicity and hydrophobicity on the surfaces of the prepared high hydrophobic aerogel composite materials or composite aerogel composite materials can broaden the application areas of the products. Therefore, the hydrophobic aerogel composite materials or composite aerogel composite materials prepared by this technique are relatively easy to combine or coat with other substrates.

[0043] 3. In this invention, the traditional sol-gel synthesis technology is improved and combined with direct suspension dispersion technology. The preparation process does not require the addition of a large amount of organic solvents and surfactants. Therefore, the process can produce high-purity, low-cost aerogel composite materials with low thermal conductivity without the need for subsequent water washing. The developed product has superior properties and high temperature resistance. The application temperature range of the developed product can be increased from 200°C to nearly 1250°C. Furthermore, it is less likely to release odors and toxic gases under high-temperature applications.

[0044] 4. Traditionally, aerogel composite products prepared using pure tetramethylsiloxane, such as tetramethylsiloxane, or hydrophobically modified methylsiloxane, such as methyltrimethylsiloxane, under normal pressure drying without hydrophobic organic solvents, are generally non-crystalline siloxane aggregates with no porosity. Similar to water glass, although its density is extremely light, its thermal insulation properties at high temperatures cannot be compared with those of aerogels with a large number of pores.

[0045] 5. In this invention, by utilizing different proportions of siloxane compounds or methylsiloxane compounds, the water content of the hydrolysis or condensation reaction, the suspended dispersion water content, the acid catalyst and alkali catalyst content, and the stirring rate of the suspension dispersion, the microstructure, porosity, pore size and distribution, aerogel particle size and distribution, aerogel surface structure, and hydrophilic / hydrophobic properties of the aerogel can be easily controlled. The thermal insulation properties of the prepared aerogel can be further controlled to improve its practicality.

[0046] 6. In the preparation method of the present invention, atmospheric pressure drying technology is used during the solvent drying process. This drying technology includes azeotropic distillation and solvent scalding. Azeotropic distillation drying utilizes the two-phase azeotropic principle of the mixed solvent to distill alcohol or water molecules in the wet aerogel suspension at the azeotropic temperature. The scalding step is when the trace amounts of water molecules remaining inside the semi-dry aerogel rapidly scald to form a high positive pressure. This high positive pressure is used to inhibit the shrinkage of the aerogel on the one hand, and on the other hand, to promote the formation of a large number of nano- to micro-sized micropores in the aerogel aggregate structure.

[0047] 7. In the preparation method of the present invention, during the solvent drying process, a large amount of alcohol-containing aqueous solution in the molded structure is rapidly azeotropically vaporized, and the vaporized vapor is guided to a heat exchange device for solvent recovery. The purpose of this recovery and reuse is, on the one hand, to recover the solvent used in the hydrolysis and condensation reactions; on the other hand, to recover valuable alcohol by-products to reduce manufacturing costs; and on the other hand, to recover alcohols to reduce pollution and hazards to the process space environment. Attached Figure Description

[0048] Figure 1 This is a schematic diagram of the process steps for manufacturing low-dielectric, low-thermal-conductivity aerogel composite materials according to an embodiment of the present invention.

[0049] Figure 2 Photographs of the appearance of the low dielectric and low thermal conductivity aerogel / fiberglass blanket prepared for the first embodiment of the present invention.

[0050] Figure 3 The image is a scanning electron microscope micrograph of a low-dielectric, low-thermal-conductivity aerogel / glass fiber blanket prepared in the first embodiment of the present invention, with a magnification of 250x.

[0051] Figure 4 The image is a scanning electron microscope micrograph of a low-dielectric, low-thermal-conductivity aerogel / glass fiber blanket prepared in the first embodiment of the present invention, with a magnification of 15,000x.

[0052] Figure 5 Photographs of the appearance of the low dielectric and low thermal conductivity aerogel / ceramic fiber blanket prepared for the second embodiment of the present invention.

[0053] Figure 6 Electron microscope micrograph of the low dielectric and low thermal conductivity aerogel / ceramic fiber blanket prepared for the second embodiment of the present invention, magnified 250 times.

[0054] Figure 7 Electron microscope micrograph of a low dielectric and low thermal conductivity aerogel / ceramic fiber blanket prepared for the second embodiment of the present invention, magnified 3,000 times.

[0055] Figure 8 Photograph of the appearance of the low dielectric and low thermal conductivity aerogel / polypropylene fiber mixed cellulose fiber nonwoven fabric prepared for the third embodiment of the present invention.

[0056] Figure 9 Electron microscope micrograph of a low dielectric and low thermal conductivity aerogel / polypropylene fiber mixed cellulose fiber nonwoven fabric prepared for the third embodiment of the present invention, with a magnification of 250x.

[0057] Figure 10 Electron microscope micrograph of a low dielectric and low thermal conductivity aerogel / polypropylene fiber mixed cellulose fiber nonwoven fabric prepared for the third embodiment of the present invention, with a magnification of 3000x. Detailed Implementation

[0058] Please see Figure 1 This invention discloses a method for preparing low-dielectric, low-thermal-conductivity aerogel composites, comprising the following steps: a mixing and hydrolysis step (S1), a suspension and dispersion condensation solution step (S2), a composite molding step (S3), and a solvent recovery and drying step (S4), wherein:

[0059] The mixed hydrolysis step (S1) involves mixing a siloxane compound or a methylsiloxane compound with a large amount of alcohol-containing aqueous solution to form a homogeneous mixed aqueous solution. The siloxane compound is one or more substances selected from the group consisting of tetramethoxysilane (TMOS) and tetraethoxysilane (TEOS), while the methylsiloxane compound is one or more substances selected from the group consisting of hydrophobic methyltrimethoxysilane (MTMS) and methyltriethoxysilane (MTES). The purpose of adding the methylsiloxane compound is to provide strong hydrophobic properties to the composite aerogel material; the purpose of adding the siloxane compound is to regulate the internal microstructure of the aerogel system; and the purpose of adding the alcohol-containing aqueous solution is to increase the porosity of the aerogel structure. In the overall mixed solution, the total volume percentage of siloxane compounds and methylsiloxane compounds is between 2.0 and 40.0%, while the volume percentage of the aqueous alcohol solution is between 98.0 and 60.0%. The volume ratio of siloxane compounds to methylsiloxane compounds ranges from 0:100 to 40:55, with a preferred ratio of 20:80 in this embodiment.

[0060] The aqueous solution containing trace amounts of alcohol in the mixed hydrolysis step (S1) may be a mixed solvent consisting of one or a combination of the following: process-recovered alcohols, newly added pure alcohols, process-recovered water, deionized water, distilled water, double-distilled water, anhydrous alcohols, or combinations thereof. In the aqueous solution containing trace amounts of alcohol, the molar ratio of alcohol to water ranges from 0:100 to 90:10, and in this embodiment, the preferred condition is 25:75.

[0061] The mixed hydrolysis step (S1) involves a hydrolysis reaction occurring in a mixture of a large amount of deionized water containing a trace amount of acid catalyst. The molar ratio of the total content of the siloxane compound and methylsiloxane compound mixture to the acid catalyst content is between 1:0.02 and 1:0.0005. A higher acid catalyst content in the siloxane compound and methylsiloxane compound mixture results in a faster hydrolysis rate. Furthermore, at lower acid catalyst content levels, increasing the temperature of the hydrolysis solution can also increase the hydrolysis rate. In this embodiment, the preferred conditions are a molar ratio of the total content of the siloxane compound and methylsiloxane compound mixture to the acid catalyst content of 1:0.001 and a hydrolysis temperature of 58°C.

[0062] The suspension dispersion condensation solution step (S2) involves: firstly, preparing the required alkaline catalyst aqueous solutions for the siloxane compound and methylsiloxane compound respectively; after the hydrolysis of the mixed aqueous solution of the siloxane compound and methylsiloxane compound is completed, adding a large amount of alcohol-containing dispersion aqueous solution and a trace amount of alkaline catalyst aqueous solution to the mixed hydrolysate solution of the siloxane compound and methylsiloxane compound respectively, and rapidly stirring with dispersing equipment such as emulsifiers and homogenizers to suspend and disperse the mixed hydrolysate solution in the large amount of dispersion aqueous solution, and a condensation reaction occurs during the suspension dispersion process. Under these conditions, the suspended and dispersed hydrolysate solution is dispersed into nano- to micron-sized fine water droplets, and the siloxane compound and methylsiloxane compound molecules undergo a condensation reaction in these water droplets, causing the siloxane compound and methylsiloxane compound to condense and form a suspension dispersion condensation solution, and agglomerating and condensing into an interconnected local network structure within the nano- to micron-sized fine water droplets.

[0063] In this condensation step, increasing the temperature significantly shortens the condensation reaction time (i.e., the gelation time of the aerogel). Specifically, when the weight ratio of the base catalyst to the acid catalyst is 0.85:1.0, the gelation time at room temperature (30°C) is approximately 126 minutes, and at 50°C, the gelation time is approximately 20 minutes. In the condensation reaction, the molar ratio of the base catalyst to the acid catalyst is between 0.7:1 and 1.8:1. Furthermore, in the mixed solution of the base catalyst and water, increasing the content of the base catalyst also significantly shortens the condensation reaction time. Additionally, increasing the temperature of both the hydrolysis and condensation reactions also helps to increase the reaction rates of hydrolysis and condensation. When the volume ratio of 1M alkaline catalyst to 1M acid catalyst is 0.8:1.0, the gelation time is about 360 minutes, but the dielectric loss of the aerogel will decrease. When the volume ratio of 1M alkaline catalyst to 1M acid catalyst is 1.2:1.0, the gelation time decreases to about 20 minutes. Therefore, the time of the condensation step can be controlled by temperature and the volume ratio of 1M alkaline catalyst to 1M acid catalyst.

[0064] The suspension dispersion condensation solution step (S2) involves adding a large amount of dispersion aqueous solution to the mixed hydrolysis solution of the siloxane compound and the methylsiloxane compound. The dispersion aqueous solution contains a large amount of process recycled water, deionized water, distilled water, double-distilled water, and trace amounts of newly added alcohols, process recycled alcohols, or combinations thereof. The molar ratio of alcohols to water in the dispersion aqueous solution ranges from 0:100 to 90:10, with a preferred ratio of 25:75 in this embodiment.

[0065] The suspension dispersion condensation solution step (S2) involves mixing the siloxane compound and the methylsiloxane compound in a hydrolysis solution for a condensation reaction. The volume ratio of the siloxane compound condensation solution to the methylsiloxane compound condensation solution can be from 0:100 to 90:10, and the mixture is stirred to form a homogeneous condensation mixture. This condensation solution mixing step can be divided into multiple mixing steps, such as one-stage mixing or two-stage mixing. In this mixing step, the molar ratio of the siloxane compound and the methylsiloxane compound, as well as the conditions for one-stage and two-stage mixing of the condensation solution, can control the microstructure of the aerogel product.

[0066] The suspension dispersion condensation solution step (S2) involves the following: While the condensation reaction continues in the mixture of the siloxane compound and the methylsiloxane compound condensation solution, the condensation mixture can be rapidly suspended and dispersed into a wet suspension using dispersion equipment such as an emulsifier, homogenizer, or vortex mixer in a suitable aqueous dispersion solution, such as an alcohol-containing aqueous dispersion. This disperses the developed siloxane compound and methylsiloxane compound condensation solution into a suspension dispersion condensation solution with a particle size ranging from approximately several nanometers to several thousand micrometers. During this stage, the local network structures of the siloxane compounds and methylsiloxane compounds in the siloxane compound condensation solution and the methylsiloxane compound condensation solution further interconnect to form a three-dimensional network structure. Therefore, this suspension dispersion step mainly controls the fine structure, particle size, and particle size distribution of the developed aerogel.

[0067] In the composite molding step (S3): the suspended dispersion condensation solution is then subjected to pressure suction, impregnation, or spraying techniques with various fiber blankets, fiber cloths, and fiber mats. For example, the suspended dispersion condensation solution is subjected to pressure suction impregnation under vacuum conditions, which promotes the rapid absorption of the suspended dispersion condensation solution into the fiber substrate. This causes the hydrolyzed siloxane compounds and hydrophobic siloxane molecules to condense and aggregate in the fiber blanket, forming aerogel aggregate structures of nanometer to submicron size. Subsequently, these aggregates in the fiber substrate to form a three-dimensional network gel structure, thus forming an aerogel / fiber composite material. In this aerogel / fiber composite substrate structure, the content of alcohol-containing aqueous solution in the hydrolysis solution represents the pore content within the aerogel aggregate structure; additionally, the content of the large amount of dispersed aqueous solution added in the condensation reaction represents the pore content between or outside the aerogel network structure in the aerogel / fiber composite substrate structure. Therefore, in this technology, the aerogel structure inside the aerogel composite material and the porosity in the aerogel / fiber composite substrate structure can be controlled by using the aqueous solution containing only trace amounts of alcohol and no hydrophobic organic solvents added in the hydrolysis and condensation reactions. In another embodiment, the suspended dispersion sol solution can also be injected into the continuous fiber blanket by directly using pressure impregnation technology combined with continuous process technology, so that the nano- to sub-micron-sized hydrolyzed siloxane molecules and hydrophobic siloxane molecules suspended dispersion condensation solution are injected into the continuous fiber blanket, and the gelation time is controlled to promote the interaction between the sol solution and the fiber material in a very short time, forming a wet aerogel blanket structure with a stable appearance. Subsequently, the wet aerogel blanket structure is rolled up or cut into a specific length and dried.

[0068] In the composite molding step (S3), the fiber substrate includes inorganic fibers, liquid crystal fibers, organic fibers, specifically, such as glass fibers, carbon fibers, quartz fibers, ceramic fibers, rock wool fibers, Kevlar polyamide fibers, Nomex polyamide fibers, PI polyimide fibers, nylon fibers, polyester fibers, polyethylene fibers, polypropylene fibers, cellulose fibers, and modified cellulose fibers, or a combination of two or more of these, in the form of a blanket, cloth, or mat.

[0069] In this composite molding step (S3), a bottom (or top) vacuum device can be combined with impregnation, pressure suction, spraying, spraying and other technologies to accelerate the injection of the suspended dispersion condensation solution into the fiber-containing substrate for composite molding.

[0070] The solvent recovery and drying step (S4) involves the following steps: After the suspended aerogel colloid within the aerogel / fiber composite substrate structure stabilizes, a solvent recovery and drying step is performed. This step includes a solvent azeotropic vaporization step and a solvent scalding step. In the solvent azeotropic vaporization step, the aerogel system is first placed in a high temperature environment, such as between 70 and 115 degrees Celsius. This causes a large amount of alcohol-containing aqueous solution in the aerogel system to undergo solvent azeotropic evaporation at high temperature, rapidly distilling out and recovering the alcohol-water molecules for reuse, drying the aerogel to a semi-dry state within the aerogel / fiber composite substrate. Subsequently, a solvent scalding step is performed at an even higher temperature, raising the temperature of the semi-dry aerogel particle system to a high-temperature environment of 120 to 150 degrees Celsius. This causes a rapid scalding of the trace amount of solvent contained within the aerogel / fiber composite substrate. This rapid scalding generates a high positive pressure within the aerogel, which is used to suppress shrinkage of the aerogel during the drying process. On the other hand, this positive pressure is used to induce a large number of nano- to micro-sized pores in the aerogel / fiber composite substrate and make the aerogel porous, thus enabling the preparation of a low-density and high-porosity high-thermal-insulation aerogel / fiber composite substrate.

[0071] Furthermore, since no large amounts of hydrophobic organic solvents such as alkanes, aromatic benzenes, and halogenated alkanes are added, the drying process is relatively safe, and the recovery of solvents does not require fractionation equipment, thus reducing recovery costs. Moreover, because no surfactants or ammonia are added, aerogel products with higher purity can be prepared. Because the prepared high-porosity aerogel composite material is free of impurities, the product exhibits superior thermal conductivity, dielectric constant, and dielectric loss properties. Please refer to [link / reference]. Figure 2 The image shown is an appearance photograph of the aerogel / glass fiber blanket prepared by the aforementioned preparation method in the first embodiment, which possesses properties of high purity, low cost, and low thermal conductivity. The low dielectric and low thermal conductivity aerogel / glass fiber blanket prepared using this technology has a white, blanket-like appearance, indicating that the prepared product is free of other impurities such as metal oxides. Please refer to... Figure 3 The image shows a 250x magnified scanning electron microscope (SEM) image of the aerogel / glass fiber blanket prepared by the aforementioned method in the first embodiment, exhibiting both low dielectric constant and low thermal conductivity. The image reveals the aerogel filling and structural appearance within the glass fiber tissue structure of the aerogel / glass fiber blanket. Further details can be found in the image below. Figure 4 This image shows a 15,000x magnified scanning electron microscope (SEM) image of a low-dielectric, low-thermal-conductivity aerogel / glass fiber blanket prepared using this technique. The image reveals a tightly bonded structure between the aerogel and glass fiber, with the aerogel particles on the glass fiber surface exhibiting uniform spherical structures ranging in size from tens to hundreds of nanometers, covering the outer surface of the glass fiber. Figure 4 It can be seen that the aerogel aggregate structure contains a large number of micropores.

[0072] The solvent recovery and drying step (S4) involves drying the solid aerogel wet gel structure at high temperature under normal pressure and molding drying temperature to obtain a uniform aerogel preformed composite material with low thermal conductivity; in some embodiments, the drying temperature is between 60 and 150°C.

[0073] Furthermore, the drying step includes a solvent vaporization step (S4-1) and a solvent boiling step (S4-2).

[0074] Vaporization step (S4-1): The preformed aerogel wet gel system is placed in an environment with a solvent vaporization temperature. At the same time, the preformed aerogel wet gel system is kept under normal pressure. The temperature is used to rapidly azeotropically vaporize a large number of alcohol and water molecules to dry the alcohol and water molecules in the aerogel wet gel system. In some embodiments, the vaporization temperature is 60-110°C.

[0075] S4-2: The ambient temperature of the pre-formed aerogel containing trace amounts of solvent, after vaporization, is adjusted to the solvent's boiling point, causing the trace amounts of solvent inside to rapidly vaporize and boil. In some embodiments, this boiling point is 110–150°C. It should be further noted that the high-temperature environment created by this boiling point causes the boiling phenomenon generated by the trace amounts of alcohol and water molecules inside the aerogel, resulting in positive pressure inside the aerogel. This positive pressure can suppress the shrinkage or collapse of the aerogel structure during drying. On the other hand, this positive pressure causes the aerogel network structure to expand and become porous. Therefore, this preparation method can be used to prepare low-density and high-porosity aerogels or aerogel / fiber composites with a thermal conductivity k of approximately 0.023–0.038 W / mK.

[0076] The solvent recovery and drying step (S4) involves the following steps: After the solid aerogel wet gel structure stabilizes, under normal pressure and at the azeotropic temperature of the mixed solvent at the molding drying temperature, a large amount of alcohol-containing aqueous solution in the molded structure is rapidly azeotropically vaporized, and the vaporized vapor is guided to a heat exchange device. In this plate heat exchange device, the alcohol-containing aqueous solution is condensed and recycled. In some embodiments of the invention, the condensed and recovered alcohol-containing aqueous solution is the raw material used for hydrolysis and suspension dispersion in this process, thus reducing the amount of raw materials used and lowering product manufacturing costs. Furthermore, the purpose of this recovery is to recover valuable alcohol byproducts to increase product revenue. Another purpose of recovering the alcohol-containing aqueous solution is to reduce the pollution and hazards of alcohol solvents to the environment and air during the process.

[0077] Please see Figure 5The second embodiment shows the appearance of the aerogel / ceramic fiber blanket with low dielectric and low thermal conductivity prepared by the aforementioned preparation method. The aerogel / ceramic fiber blanket prepared using this technology has a grayish-white, heat-insulating blanket-like appearance. The grayish-white color indicates the appearance color of the ceramic fibers. Further, please refer to... Figure 6 This image shows a 250x magnified scanning electron microscope (SEM) photograph of an aerogel / ceramic fiber blanket prepared by the aforementioned preparation method according to the second embodiment of this technology. The photograph reveals the aerogel filling and structural appearance within the aerogel / ceramic fiber blanket's internal fiber structure. Further details can be found in the image. Figure 7 The image shows a 3,000x magnified scanning electron microscope (SEM) image of the aerogel / ceramic fiber blanket prepared by the aforementioned preparation method in the second embodiment of this technology. The image also shows that the aerogel and ceramic fiber exhibit a tightly bonded structure, and the aerogel on the ceramic fiber surface is a uniform spherical structure ranging from approximately tens to approximately one hundred nanometers in size, covering the glass fiber exterior. Figure 7 It can be seen that the aerogel aggregates contain a large number of micropores.

[0078] Please see Figure 8 The image shows the appearance of the aerogel / polypropylene fiber mixed with cellulose fiber nonwoven fiber mat prepared by the aforementioned preparation method in the third embodiment, which possesses the properties of high purity, low cost, and low thermal conductivity. Figure 8 The aerogel / polypropylene fiber mixed with cellulose fiber nonwoven fabric mat is a product with a thickness of approximately 100 to 200 micrometers. Depending on the aerogel formulation, the aerogel / nonwoven fabric mat may be white or transparent. For further details, please refer to [link to relevant documentation]. Figure 9 This image shows a 250x magnified scanning electron microscope (SEM) photograph of a portion of the aerogel / polypropylene fiber mixed cellulose fiber nonwoven fabric mat prepared by the aforementioned preparation method in the third embodiment of this technology. The photograph reveals the filling morphology of the aerogel between the nonwoven fiber structures within the aerogel / polypropylene fiber mixed cellulose fiber nonwoven fabric mat. Further details can be found in the attached image. Figure 10 The image shows a 3,000x magnified scanning electron microscope image of the aerogel / polypropylene fiber mixed cellulose fiber non-woven fabric prepared by the aforementioned preparation method in the third embodiment of this technology. The image also shows that the size of the aerogel between the non-woven structures is a uniform spherical structure between about tens to about one hundred nanometers, stacked between the polypropylene fiber mixed cellulose fiber non-woven fabric fibers. It can also be seen that the aerogel aggregate structure contains a large number of micropores to provide the thermal insulation effect of the aerogel / polypropylene fiber mixed cellulose fiber non-woven fabric.

[0079] The hydrophobic or hydrophobic-hydrophilic complex aerogel / fiber composites produced by this technology have densities ranging from approximately 0.25 to 0.45 g / cm³. 3 Between these two conditions, due to the absence of other impurities in the manufacturing process, the thermal conductivity is significantly reduced, with the thermal conductivity coefficient of hydrophobic aerogel / fiber composites ranging from approximately 0.019 to 0.032 W / mk.

[0080] In summary, the manufacturing, application, and effects of the present invention have been clearly disclosed. However, the above-described embodiments are only preferred embodiments of the present invention and should not be construed as limiting the scope of patent protection of the present invention. That is, simple equivalent changes and modifications made in accordance with the claims and description of the present invention all fall within the scope of patent protection of the present invention.

Claims

1. A method for preparing a low-dielectric, low-thermal-conductivity aerogel / fiber composite material, characterized in that, Includes the following steps: Mixed hydrolysis step: Siloxane compound and methylsiloxane compound are separately mixed with a large amount of aqueous solution containing trace amounts of alcohol, and a trace amount of acid catalyst is added under stirring to carry out the hydrolysis reaction in the mixed solution. The siloxane compound is tetramethoxysilane or tetraethoxysilane, and the methylsiloxane compound is methyltrimethoxysilane or methyltriethoxysilane. In the overall mixed solution, the total volume percentage of the siloxane compound and the methylsiloxane compound is between 2.0 and 40.0%, while the volume percentage of the large amount of aqueous solution containing trace amounts of alcohol is between 98.0 and 60.0%. The molar ratio of alcohol to water in the aqueous solution is 25:75, and the molar ratio of the total content of the mixture of siloxane compound and the methylsiloxane compound to the content of the trace amount of acid catalyst is 1:0.02 to 1:0.0005. Suspension dispersion condensation solution step: After the mixed solution is hydrolyzed, an alcohol-containing dispersion aqueous solution and an alkaline catalyst aqueous solution are added respectively, and the mixture is rapidly suspended and dispersed into a suspension dispersion droplet using an emulsifier or homogenizer. A condensation reaction then occurs in the droplet, causing the siloxane compound and the methylsiloxane compound to condense and form a suspension dispersion condensation solution. Composite molding steps: The suspended dispersion condensation solution is subjected to pressure suction and impregnation technology under vacuum conditions, which promotes the rapid absorption of the suspended dispersion condensation solution into the fiber substrate. This causes the hydrolyzed siloxane compounds and methylsiloxane compounds to condense and aggregate in the fiber substrate, forming nano- to sub-micron-sized aerogel wet aggregates. Subsequently, these aggregates in the fiber substrate to form a three-dimensional network gel structure, thus forming an aerogel / fiber composite material. The fiber substrate includes one or both of inorganic and organic fibers, and is in the form of a blanket, cloth, or mat. Solvent recovery and drying steps: Under normal pressure, the aerogel / fiber composite material is placed between 70 and 115 degrees Celsius, so that the large amount of water containing trace amounts of alcohol in the aerogel system undergoes azeotropic evaporation at high temperature, thereby rapidly distilling out and recovering the large amount of water containing trace amounts of alcohol for reuse. Subsequently, it is rapidly vaporized between 120 and 150 degrees Celsius to obtain a dry aerogel / fiber composite material.

2. The preparation method according to claim 1, characterized in that: The volume ratio of the siloxane compound to the methylsiloxane compound ranges from 0:100 to 40:

55.

3. The preparation method according to claim 1, characterized in that: The large volume of aqueous solution containing trace amounts of alcohol in the mixed hydrolysis step is a mixed solvent selected from one or a combination of the following groups: process recovery water, process recovery aqueous solution containing alcohol, process recovery alcohol, or pure alcohol.

4. The preparation method according to claim 1, characterized in that: In the condensation reaction, the molar ratio of the base catalyst to the acid catalyst is 0.7:1 to 1.8:

1.

5. The preparation method according to claim 1, characterized in that: In this suspension dispersion condensation solution step, when the mixed solution undergoes a condensation reaction, the mixed solution is rapidly suspended and dispersed in a suitable alcohol-containing aqueous dispersion to form a wet suspension dispersion condensation solution with a particle size of several nanometers to several thousand micrometers using an emulsifier, homogenizer or vortex mixer.

6. The preparation method according to claim 1, characterized in that: In the suspension dispersion condensation solution step, the alcohol-containing aqueous dispersion is a mixed solvent selected from one or a combination of the following groups: process recovery water, process recovery alcohol-containing aqueous solution, process recovery alcohol, or pure alcohol.

7. The preparation method according to claim 1, characterized in that: The composite molding process involves using pressure suction and impregnation techniques to rapidly draw the suspended dispersion condensation solution into the fiber substrate, where it then aggregates to form a three-dimensional network aerogel / fiber composite structure.

8. The preparation method according to claim 1, characterized in that: The solvent recovery and drying step involves the following steps: After the suspended aerogel colloid within the aerogel / fiber composite substrate structure stabilizes, a solvent recovery and drying step is performed, which includes a solvent azeotropic vaporization step and a solvent scalding step. In the solvent azeotropic vaporization step, the aerogel system is first subjected to a high-temperature azeotropic evaporation of a large amount of aqueous solution containing trace amounts of alcohol, thereby rapidly azeotropically distilling and drying the alcohol water molecules to a semi-dry aerogel within the aerogel / fiber composite substrate. Subsequently, a solvent scalding step is performed at an even higher temperature to cause a rapid scalding phenomenon of the solvent contained within the aerogel / fiber composite substrate, inhibiting the shrinkage of the aerogel during the drying process.

9. The preparation method according to claim 1, characterized in that: The sol-gel reaction modification technique is used to control the microstructure, porosity, pore size and distribution, and particle size and distribution of the developed highly hydrophobic aerogel by utilizing the content of the mixture of the siloxane compound and the methylsiloxane compound, the content of the hydrolysis solution containing trace amounts of acid catalyst, the content of the dispersion aqueous solution containing alkali catalyst, the mixing ratio and steps of the suspension dispersion condensation solution, the rapid suspension dispersion stirring rate, and specific drying temperature conditions.

Citation Information

Patent Citations

  • Low-K dielectric layer structure, semiconductor device structure and formation method thereof

    CN102044525A

  • Aerogel insulation panels and manufacturing thereof

    CN105189104A

  • Method for preparing cross-linked polyimide aerogel

    CN108203516A

  • Heat insulation member and heating assembly

    CN113873697A

  • Flexible composite aerogel and manufacturing process

    TW201542457A