An ultra-high strength high-plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy and a preparation method thereof

By preparing Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloys, the problem of decreased plasticity when increasing the strength of high-strength titanium alloys was solved, achieving a balance between high strength and high plasticity, thus meeting the requirements of the next generation of aircraft for high strength and high plasticity.

CN118028656BActive Publication Date: 2026-11-24西部超导材料科技股份有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410175088.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-07
Publication Date
2026-11-24
Estimated Expiration
2044-02-07

AI Technical Summary

Technical Problem

Existing high-strength titanium alloys exhibit a significant decrease in plasticity when their strength is increased, making it difficult to meet the high strength and high plasticity requirements of next-generation aircraft. In particular, their application in high-strength and high-plasticity service conditions, such as fasteners, is limited.

Method used

A high-strength and high-ductility titanium alloy was prepared by using Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy, through specific component ratios and strict control of impurity elements, combined with three vacuum self-consuming electric arc furnace melting, forging, rolling and solution aging treatments.

Benefits of technology

We have obtained ultra-high strength and high plasticity titanium alloys with tensile strength of over 1500MPa, elongation of over 16%, and reduction of area of ​​over 40%, which meet the high strength requirements of fasteners and other fasteners.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118028656B_ABST
    Figure CN118028656B_ABST
Patent Text Reader

Abstract

This invention discloses an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy and its preparation method. The alloy, by weight percentage, comprises 5.0–7.0% Al, 3.0–5.0% Mo, 3.0–5.0% Zr, 1.5–2.5% Sn, 1.5–3.5% Cr, 1.0–3.0% Fe, and 0.07–0.10% O, and also includes impurities. The impurity content is controlled by weight percentage as follows: C ≤ 0.01%, Si ≤ 0.01%, N ≤ 0.003%, H ≤ 0.007%, and Hf ≤ 0.05%. The preparation method includes the following steps: weighing raw materials according to the proportions of different constituent elements and mixing them thoroughly; pressing and welding the uniformly mixed raw materials into electrode blocks to form consumable electrodes, and performing three vacuum consumable arc furnace melting processes; forging, rolling, and solution aging treatment on the resulting titanium alloy ingot to obtain the ultra-high strength and high plasticity titanium alloy. This invention can obtain an ultra-high strength and high plasticity titanium alloy with high strength and high plasticity, whose tensile strength can reach more than 1500MPa, elongation can reach more than 16%, and reduction of area can reach more than 40%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-performance alloy materials technology, specifically relating to an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy and its preparation method. Background Technology

[0002] High-strength titanium alloys generally refer to titanium alloys with a tensile strength greater than 1100 MPa. In addition to high strength, they also have good plasticity, toughness and corrosion resistance, making them one of the main structural materials in the aerospace field. Currently, the commonly used alloying scheme for high-strength titanium alloys is to add a large amount of β-stabilizing elements such as Mo, V, Cr, and Fe, such as Ti-15V-3Cr-3Al-3Sn (TB5), Ti-10V-2Fe-3Al (TB6), Ti-32Mo (TB7), and Ti-5Mo-5V-2Cr-3Al (TB10). Among these titanium alloys, TB10 titanium alloy has good plasticity at 1100-1200 MPa, but further increasing the strength will cause a loss of plasticity; TB7 titanium alloy has an elongation of up to 10% when the strength is 800-1000 MPa, and its strength can reach 1300-1400 MPa under heat treatment strengthening, but its plasticity is almost lost; even the new Ti-5553 titanium alloy has an elongation of more than 16% when the strength is 1000-1058 MPa, but when its strength is >1300 MPa, the elongation is <6%, and its plasticity is severely lost.

[0003] With the advent of design concepts such as lightweighting, high reliability, and long service life, the demand for high-strength and high-ductility structural components in next-generation aircraft is becoming increasingly urgent. This requires titanium alloys to possess both higher strength and good ductility. As can be seen from the properties of existing titanium alloys, increasing the strength of high-strength titanium alloys typically leads to a loss of ductility and toughness. Some fasteners require strength indicators of 1500 MPa or even higher, while the yield strength of existing titanium alloys is generally below 1300 MPa, and ductility decreases significantly with increasing strength, severely limiting the application of structural titanium alloys in high-strength and high-ductility service conditions such as fasteners. Summary of the Invention

[0004] The purpose of this invention is to provide an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy and its preparation method, which can obtain an ultra-high strength and high plasticity titanium alloy with a tensile strength of over 1500 MPa, an elongation of over 16%, and a reduction of area of ​​over 40%.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0006] An ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy, by weight percentage, comprises 5.0–7.0% Al, 3.0–5.0% Mo, 3.0–5.0% Zr, 1.5–2.5% Sn, 1.5–3.5% Cr, 1.0–3.0% Fe, and 0.07–0.10% O, and also includes impurities, the impurity content of which is controlled by weight percentage as follows: C≤0.01%, Si≤0.01%, N≤0.003%, H≤0.007%, Hf≤0.05%.

[0007] A method for preparing ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy includes the following steps:

[0008] S1. Weigh the raw materials according to the proportions of different components and mix them thoroughly.

[0009] S2, the uniformly mixed raw materials are pressed and welded into electrode blocks to form consumable electrodes, which are then smelted in a vacuum consumable arc furnace three times.

[0010] S3. The obtained titanium alloy ingot is forged, rolled and solution aged to obtain an ultra-high strength and high plasticity titanium alloy.

[0011] Preferably, in S1, titanium is introduced as sponge titanium, zirconium is introduced as sponge zirconium, and other elements are introduced as intermediate alloys. The sponge zirconium is a combination of low-Hf sponge zirconium and industrial-grade sponge zirconium. The low-Hf sponge zirconium has an Hf of <0.5% and accounts for 20% to 50% of the total weight of sponge zirconium.

[0012] Preferably, in step S2, the three-stage vacuum consumable arc furnace melting includes the following steps:

[0013] S201, first undergo a second VAR melting process;

[0014] S202, the consumable electrode obtained by secondary VAR melting is loaded into a strongly cooled crucible and placed in the VAR furnace melting station for furnace sealing and evacuation.

[0015] S203, during the melting process, gas is injected into the gap between the melted consumable electrode and the crucible using a pressure control method. The melting voltage is 24-34V, the melting current is 8-16kA, and the arc stabilization current is 10-20A AC.

[0016] S204, when the remaining weight of the consumable electrode is 70-250kg, feeding begins and gas is injected using a flow control method. After melting, cooling is still carried out by injecting gas. Then the consumable electrode is cooled normally and removed from the furnace to finally obtain a titanium alloy ingot.

[0017] Preferably, in step S4, the forging process includes: after trimming the titanium alloy ingot, performing initial forging at a starting temperature of 1080–1200°C, holding for 90 minutes, and achieving a deformation of ≥30%; then performing a high-temperature forging + two-phase forging cycle forging, with the high-temperature forging temperature at 920–1000°C and a deformation of ≥30%, and the two-phase forging temperature at 830–860°C and a deformation of ≥20%; after the cycle forging, performing multiple hot drawing at a temperature of 820–870°C to obtain the forged billet.

[0018] Preferably, in step S4, the rolling process is as follows: multiple hot rolling passes are performed at 50–130°C below the phase transformation point, with a deformation of 71%–88%, to obtain the hot-rolled billet.

[0019] Preferably, in step S4, the solution aging process is as follows: after solution treatment at 820–880°C for 2 hours, the solution is quenched in water to room temperature, and then aged at 510–620°C for 4–8 hours followed by air cooling to obtain an ultra-high strength and high plasticity titanium alloy.

[0020] Preferably, in S4, the ultra-high strength and high plasticity titanium alloy has a tensile strength of over 1500 MPa, an elongation of over 16%, and a reduction of area of ​​over 40%.

[0021] Compared with the prior art, the present invention has the following beneficial technical effects:

[0022] (1) The present invention provides an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy, which comprises 5.0-7.0% Al, 3.0-5.0% Mo, 3.0-5.0% Zr, 1.5-2.5% Sn, 1.5-3.5% Cr, 1.0-3.0% Fe, 0.07-0.10% O, and trace amounts of impurities, C≤0.01%, Si≤0.01%, N≤0.003%, H≤0.007%, Hf≤0.05%. The various β-phase stabilizing elements selected in this alloy can effectively improve the strength of the titanium alloy, while strictly controlling the content of O and impurity elements such as C, H, N, and Hf to ensure the plasticity of the alloy.

[0023] (2) The present invention provides a method for preparing an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy, which contains 3 to 5% Zr and uses low Hf sponge zirconium + industrial-grade sponge zirconium in combination, which can effectively control the impurity elements in the alloy to <0.1%.

[0024] (3) The present invention provides a method for preparing an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy. This alloy is prepared by mixing materials, pressing electrode blocks, welding, and then undergoing three melting processes of different specifications in a vacuum consumable arc furnace to obtain highly uniform, finely grained columnar crystals. After high-temperature forging at 920–1000℃ and cyclic forging in a two-phase region at 830℃–860℃, followed by multiple direct drawing processes at 820–870℃, and then further processing... By hot rolling at 50–130°C below the change point in multiple passes, followed by solution treatment at 820–880°C for 2 hours and water quenching to room temperature, and then aging at 510–620°C for 4–8 hours followed by air cooling, an ultra-high strength and high plasticity titanium alloy can be obtained. Its tensile strength can reach over 1500 MPa, elongation can reach over 16%, and reduction of area can reach over 40%, meeting the strength requirements of 1500 MPa or even higher for some fasteners, and achieving a good match between the strength and plasticity of the alloy. Attached Figure Description

[0025] Figure 1 This is a macroscopic microstructure diagram of a Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy ingot. Detailed Implementation

[0026] To make the technical solution of the present invention clearer, the technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and embodiments.

[0027] An ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy, by weight percentage, comprises 5.0–7.0% Al, 3.0–5.0% Mo, 3.0–5.0% Zr, 1.5–2.5% Sn, 1.5–3.5% Cr, 1.0–3.0% Fe, and 0.07–0.10% O, and also includes impurities, the impurity content of which is controlled by weight percentage as follows: C≤0.01%, Si≤0.01%, N≤0.003%, H≤0.007%, Hf≤0.05%.

[0028] A method for preparing an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy includes the following steps:

[0029] S1. Weigh the raw materials according to the proportions of different components and mix them thoroughly.

[0030] In the raw materials used for alloy smelting, titanium is introduced in the form of sponge titanium, zirconium is introduced in the form of sponge zirconium, and other elements are introduced in the form of intermediate alloy. Among them, sponge zirconium is a combination of low-Hf sponge zirconium and industrial-grade sponge zirconium. The low-Hf sponge zirconium has Hf < 0.5% and accounts for 20% to 50% of the total weight of sponge zirconium.

[0031] The composition of different elements, by weight percentage, includes 5.0–7.0% Al, 3.0–5.0% Mo, 3.0–5.0% Zr, 1.5–2.5% Sn, 1.5–3.5% Cr, 1.0–3.0% Fe, and 0.07–0.10% O. It also includes impurities, the impurity content of which is controlled by weight percentage as follows: C ≤ 0.01%, Si ≤ 0.01%, N ≤ 0.003%, H ≤ 0.007%, and Hf ≤ 0.05%. The sponge zirconium is a combination of low-Hf sponge zirconium and industrial-grade sponge zirconium, with low-Hf sponge zirconium accounting for 25% of the total weight of the sponge zirconium.

[0032] The various β-phase stabilizing elements selected in this alloy can effectively improve the strength of the titanium alloy. At the same time, the content of O and impurity elements such as C, H, N, and Hf are strictly controlled to ensure the plasticity of the alloy.

[0033] Containing 3-5% Zr, and using a combination of low-Hf sponge zirconium and industrial-grade sponge zirconium, the impurity elements in the alloy can be effectively controlled to <0.1%.

[0034] S2, the uniformly mixed raw materials are pressed and welded into electrode blocks to form consumable electrodes, which are then smelted in a vacuum consumable arc furnace three times.

[0035] The uniformly mixed raw materials are pressed into electrode blocks using a large hydraulic press, protected by non-tungsten inert gas (TIG) and then welded into consumable electrodes using a plasma welding box. Different specifications are then melted three times in a vacuum consumable arc furnace.

[0036] The three-stage vacuum consumable arc furnace melting process includes the following steps:

[0037] S201, first undergo a second VAR melting process.

[0038] S202, the consumable electrode obtained by secondary VAR melting is loaded into a strongly cooled crucible and placed in the VAR furnace melting station for furnace sealing and evacuation.

[0039] S203, during the smelting process, gas is injected into the gap between the melted consumable electrode and the crucible using a pressure control method. The smelting voltage is 24-34V, the smelting current is 8-16kA, and the arc stabilizing current is 10-20A AC.

[0040] S204, when the remaining weight of the consumable electrode is 70-250kg, feeding begins and gas is injected using a flow control method. After melting, cooling is still carried out by injecting gas. Then the consumable electrode is cooled normally and removed from the furnace to finally obtain a titanium alloy ingot.

[0041] The titanium alloy ingot is a large-sized ingot with highly uniform, significantly refined, columnar grains.

[0042] S3. The obtained titanium alloy ingot is forged, rolled and solution aged to obtain an ultra-high strength and high plasticity titanium alloy.

[0043] The forging process includes: after trimming the titanium alloy ingot, it is forged at a forging temperature of 1080-1200℃, held for 90 minutes, and the deformation is ≥30%; then it undergoes high-temperature forging + two-phase zone forging cyclic forging, with the high-temperature forging temperature at 920-1000℃ and the deformation being ≥30%, and the two-phase zone forging temperature at 830-860℃ and the deformation being ≥20%; after cyclic forging, it is drawn in multiple passes at a temperature of 820-870℃ to obtain the forged billet.

[0044] The rolling process is as follows: multiple hot rolling passes are performed at 50 to 130°C below the phase transformation point, with a deformation of 71% to 88%, to obtain the hot-rolled billet.

[0045] The solution aging process is as follows: after solution treatment at 820-880℃ for 2 hours, the solution is quenched in water to room temperature, and then aged at 510-620℃ for 4-8 hours before air cooling to obtain an ultra-high strength and high plasticity titanium alloy.

[0046] Ultra-high strength and high plasticity titanium alloys combine high strength and high plasticity. Their tensile strength can reach more than 1500MPa, elongation can reach more than 16%, and reduction of area can reach more than 40%.

[0047] The present invention will be further described in detail through the following embodiments.

[0048] Example 1

[0049] An ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy, by weight percentage, comprises 6.0–6.5% Al, 3.0–4.0% Mo, 3.0–4.0% Zr, 1.5–2.0% Sn, 1.5–2.5% Cr, 1.0–2.0% Fe, 0.07–0.10% O, and trace amounts of impurities, C≤0.01%, Si≤0.01%, N≤0.003%, H≤0.007%, Hf≤0.05%.

[0050] A method for preparing an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy includes the following steps:

[0051] S1. Weigh the raw materials according to the proportions of different components and mix them thoroughly.

[0052] In the raw materials used for alloy smelting, titanium is introduced in the form of sponge titanium, zirconium is introduced in the form of sponge zirconium, and other elements are introduced in the form of intermediate alloy. Among them, sponge zirconium is a combination of low Hf sponge zirconium and industrial grade sponge zirconium, with low Hf sponge zirconium accounting for 25% of the total weight of sponge zirconium.

[0053] The composition of different elements, by weight percentage, includes 6.0–6.5% Al, 3.0–4.0% Mo, 3.0–4.0% Zr, 1.5–2.0% Sn, 1.5–2.5% Cr, 1.0–2.0% Fe, and 0.07–0.10% O. It also includes impurities, the impurity content of which is controlled by weight percentage as follows: C≤0.01%, Si≤0.01%, N≤0.003%, H≤0.007%, and Hf≤0.05%.

[0054] S2, the uniformly mixed raw materials are pressed and welded into electrode blocks to form consumable electrodes, which are then smelted in a vacuum consumable arc furnace three times.

[0055] The uniformly mixed raw materials are pressed into electrode blocks using a large hydraulic press, protected by non-tungsten inert gas (TIG) and then welded into consumable electrodes using a plasma welding box. Different specifications are then melted three times in a vacuum consumable arc furnace.

[0056] The three-stage vacuum consumable arc furnace melting process includes the following steps:

[0057] S201, first undergo a second VAR melting process.

[0058] S202, the consumable electrode obtained by secondary VAR melting is loaded into a strongly cooled crucible and placed in the VAR furnace melting station for furnace sealing and evacuation.

[0059] S203, during the melting process, gas is injected into the gap between the melted consumable electrode and the crucible using a pressure control method. The melting voltage is 28V, the melting current is 8kA, and the arc stabilization current is 10-20A AC.

[0060] S204, when the remaining weight of the consumable electrode is 70-250kg, feeding begins and gas is injected using a flow control method. After melting, cooling is still carried out by injecting gas. Then the consumable electrode is cooled normally and removed from the furnace to finally obtain a titanium alloy ingot.

[0061] The titanium alloy ingot is a large-sized ingot with highly uniform, significantly refined, columnar grains.

[0062] S3. The obtained titanium alloy ingot is forged, rolled and solution aged to obtain an ultra-high strength and high plasticity titanium alloy.

[0063] The forging process includes: after trimming the titanium alloy ingot, it is forged at 1080℃, then forged at 980℃ and 830℃ in the two-phase zone, respectively. The forging is carried out in a cycle of high temperature and two-phase zone, and then the forged billet is drawn in 4 heats at 825℃.

[0064] The rolling process is as follows: the forged billet is hot rolled in multiple passes at 80°C below the phase transformation point, with a cumulative deformation of 71% to 88%, to obtain the hot-rolled billet.

[0065] The solution aging process is as follows: after hot rolling, the billet is solution-treated at 840℃ for 2 hours, then water-quenched to room temperature, aged at 540℃ for 6 hours, and then air-cooled to obtain an ultra-high strength and high plasticity titanium alloy.

[0066] The organizational features of this embodiment are as follows: Figure 1 As shown in Table 1, the composition is as shown in Example 1, and the measured mechanical properties of the alloy are as shown in Table 2, Example 1.

[0067] Table 1 Chemical composition of different embodiments of Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy

[0068]

[0069] Table 2 Mechanical properties of different embodiments of Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy

[0070]

[0071] Example 2

[0072] An ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy, by weight percentage, comprises 5.0–6.0% Al, 4.0–5.0% Mo, 4.0–4.5% Zr, 2.0–2.5% Sn, 2.5–3.0% Cr, 2.0–3.0% Fe, and 0.07–0.10% O, and also includes impurities, the impurity content of which is controlled by weight percentage as follows: C≤0.01%, Si≤0.01%, N≤0.003%, H≤0.007%, Hf≤0.05%.

[0073] A method for preparing an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy includes the following steps:

[0074] S1. Weigh the raw materials according to the proportions of different components and mix them thoroughly.

[0075] In the raw materials used for alloy smelting, titanium is introduced in the form of sponge titanium, zirconium is introduced in the form of sponge zirconium, and other elements are introduced in the form of intermediate alloy. Among them, sponge zirconium is a combination of low Hf sponge zirconium and industrial grade sponge zirconium, with low Hf sponge zirconium accounting for 35% of the total weight of sponge zirconium.

[0076] The composition of different elements, by weight percentage, includes 5.0–6.0% Al, 4.0–5.0% Mo, 4.0–4.5% Zr, 2.0–2.5% Sn, 2.5–3.0% Cr, 2.0–3.0% Fe, and 0.07–0.10% O. It also includes impurities, the impurity content of which is controlled by weight percentage as follows: C≤0.01%, Si≤0.01%, N≤0.003%, H≤0.007%, and Hf≤0.05%.

[0077] S2, the uniformly mixed raw materials are pressed and welded into electrode blocks to form consumable electrodes, which are then smelted in a vacuum consumable arc furnace three times.

[0078] S3, the uniformly mixed raw materials are pressed into electrode blocks using a large hydraulic press, protected by non-tungsten inert gas (TIG) and then welded into consumable electrodes using a plasma welding box; different specifications are then melted three times in a vacuum consumable arc furnace.

[0079] The three-stage vacuum consumable arc furnace melting process includes the following steps:

[0080] S201, first undergo a second VAR melting process.

[0081] S202, the consumable electrode obtained by secondary VAR melting is loaded into a strongly cooled crucible and placed in the VAR furnace melting station for furnace sealing and evacuation.

[0082] S203, during the melting process, gas is injected into the gap between the melted consumable electrode and the crucible using a pressure control method. The melting voltage is 30V, the melting current is 10kA, and the arc stabilization current is 10-15A AC.

[0083] S204, when the remaining weight of the consumable electrode is 70-250kg, feeding begins and gas is injected using a flow control method. After melting, cooling is still carried out by injecting gas. Then the consumable electrode is cooled normally and removed from the furnace to finally obtain a titanium alloy ingot.

[0084] The titanium alloy ingot is a large-sized ingot with highly uniform, significantly refined, columnar grains.

[0085] S3. The obtained titanium alloy ingot is forged, rolled and solution aged to obtain an ultra-high strength and high plasticity titanium alloy.

[0086] The forging process includes: after trimming the titanium alloy ingot, it is forged at 1100℃, then forged at 1000℃ and 840℃ in the two-phase zone, respectively, and forged by cyclic forging in the high temperature + two-phase zone. Finally, it is drawn in 4 heats at 830℃ to obtain the forged billet.

[0087] The rolling process is as follows: the forged billet is hot rolled in multiple passes at 90°C below the phase transformation point, with a cumulative deformation of 71% to 88%, to obtain the hot-rolled billet.

[0088] The solution aging process is as follows: after hot rolling, the billet is solution-treated at 850℃ for 2 hours, then water-quenched to room temperature, aged at 550℃ for 6 hours, and then air-cooled to obtain an ultra-high strength and high plasticity titanium alloy.

[0089] The composition of this embodiment is shown in Table 1, Example 2, and the measured mechanical properties of the alloy are shown in Table 2, Example 2.

[0090] Example 3

[0091] An ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy, by weight percentage, comprises 6.5–7.0% Al, 4.5–5.0% Mo, 4.5–5.0% Zr, 2.0–2.5% Sn, 3.0–3.5% Cr, 2.0–3.0% Fe, and 0.07–0.10% O, and also includes impurities, the impurity content of which is controlled by weight percentage as follows: C≤0.01%, Si≤0.01%, N≤0.003%, H≤0.007%, Hf≤0.05%.

[0092] A method for preparing an ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy includes the following steps:

[0093] S1. Weigh the raw materials according to the proportions of different components and mix them thoroughly.

[0094] In the raw materials used for alloy smelting, titanium is introduced in the form of sponge titanium, zirconium is introduced in the form of sponge zirconium, and other elements are introduced in the form of intermediate alloy. Among them, sponge zirconium is a combination of low Hf sponge zirconium and industrial grade sponge zirconium, with low Hf sponge zirconium accounting for 45% of the total weight of sponge zirconium.

[0095] The composition of different elements, by weight percentage, includes 6.5–7.0% Al, 4.5–5.0% Mo, 4.5–5.0% Zr, 2.0–2.5% Sn, 3.0–3.5% Cr, 2.0–3.0% Fe, and 0.07–0.10% O. It also includes impurities, the impurity content of which is controlled by weight percentage as follows: C ≤ 0.01%, Si ≤ 0.01%, N ≤ 0.003%, H ≤ 0.007%, and Hf ≤ 0.05%.

[0096] S2, the uniformly mixed raw materials are pressed and welded into electrode blocks to form consumable electrodes, which are then smelted in a vacuum consumable arc furnace three times.

[0097] The uniformly mixed raw materials are pressed into electrode blocks using a large hydraulic press, protected by non-tungsten inert gas (TIG) and then welded into consumable electrodes using a plasma welding box. Different specifications are then melted three times in a vacuum consumable arc furnace.

[0098] The three-stage vacuum consumable arc furnace melting process includes the following steps:

[0099] S201, first undergo a second VAR melting process.

[0100] S202, the consumable electrode obtained by secondary VAR melting is loaded into a strongly cooled crucible and placed in the VAR furnace melting station for furnace sealing and evacuation.

[0101] S203, during the melting process, gas is injected into the gap between the melted consumable electrode and the crucible using a pressure control method. The melting voltage is 32V, the melting current is 12kA, and the arc stabilization current is 15~18A AC.

[0102] S204, when the remaining weight of the consumable electrode is 70-250kg, feeding begins and gas is injected using a flow control method. After melting, cooling is still carried out by injecting gas. Then the consumable electrode is cooled normally and removed from the furnace to finally obtain a titanium alloy ingot.

[0103] The titanium alloy ingot is a large-sized ingot with highly uniform, significantly refined, columnar grains.

[0104] S3. The obtained titanium alloy ingot is forged, rolled and solution aged to obtain an ultra-high strength and high plasticity titanium alloy.

[0105] The forging process includes: after trimming the titanium alloy ingot, it is forged at 1120℃, then forged at 990℃ and 850℃ in the two-phase zone, respectively, and the forging is carried out in a cycle of high temperature and two-phase zone. Finally, it is drawn in 4 heats at 830℃ to obtain the forged billet.

[0106] The rolling process is as follows: the forged billet is hot rolled in multiple passes at 100°C below the phase transformation point, with a cumulative deformation of 71% to 88%, to obtain the hot-rolled billet.

[0107] The solution aging process is as follows: after hot rolling, the billet is solution-treated at 860℃ for 2 hours, then water-quenched to room temperature, aged at 560℃ for 6 hours, and then air-cooled to obtain an ultra-high strength and high plasticity titanium alloy.

[0108] The composition of this embodiment is shown in Table 1, Example 3, and the measured mechanical properties of the alloy are shown in Table 2, Example 3.

[0109] Comparative Example 1

[0110] The ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy obtained by the method in Example 1 was subjected to performance testing directly without heat treatment in its forged state.

[0111] The composition of this comparative example is shown in Comparative Example 1 in Table 1, and the measured mechanical properties of the alloy are shown in Comparative Example 1 in Table 2.

[0112] Comparative Example 2

[0113] An ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy was prepared, comprising, by weight percentage, 4.5–4.8% Al, 5.2–5.8% Mo, 5.2–5.8% Zr, 2.6–2.9% Sn, 0.5–1.5% Cr, 0.2–1.0% Fe, 0.11–0.18% O, with the balance being Ti.

[0114] The Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy prepared by the method in Example 1 was solution-treated in the two-phase region at 850-880℃ for 2 hours, then water-quenched to room temperature, and finally aged at 500-600℃ for 4-8 hours.

[0115] The composition of this comparative example is shown in Table 1 (Comparative Example 2), and the measured mechanical properties of the alloy are shown in Table 2 (Comparative Example 2).

Claims

1. A high-strength, high-plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy, characterized in that, By weight percentage, it includes 5.0–7.0% Al, 3.0–5.0% Mo, 3.0–5.0% Zr, 1.5–2.5% Sn, 1.5–3.5% Cr, 1.0–3.0% Fe, 0.07–0.10% O, with the balance being Ti and impurities. The impurity content is controlled by weight percentage as follows: C ≤ 0.01%, Si ≤ 0.01%, N ≤ 0.003%, H ≤ 0.007%, Hf ≤ 0.05%. The titanium alloy is prepared by the following method: S1. Weigh the raw materials according to the proportions of different components and mix them thoroughly. In S1, titanium is introduced as sponge titanium, zirconium is introduced as sponge zirconium, and other elements are introduced as intermediate alloys. Among them, sponge zirconium is a combination of low-Hf sponge zirconium and industrial-grade sponge zirconium. The low-Hf sponge zirconium has an Hf of <0.5% and accounts for 20% to 50% of the total weight of sponge zirconium. S2, the uniformly mixed raw materials are pressed and welded into electrode blocks to form consumable electrodes, which are then smelted in a vacuum consumable arc furnace three times. S3. The obtained titanium alloy ingot is forged, rolled and solution aged to obtain an ultra-high strength and high plasticity titanium alloy. In S3, the solution aging process is as follows: after solution treatment at 820-880℃ for 2 hours, the solution is quenched in water to room temperature, and then aged at 510-620℃ for 4-8 hours followed by air cooling.

2. The ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy according to claim 1, characterized in that, In step S2, the three-stage vacuum consumable arc furnace smelting includes the following steps: S201, first undergo secondary vacuum consumable electric arc furnace smelting; S202, the consumable electrode obtained by secondary vacuum consumable arc furnace melting is loaded into a strong cooling crucible and placed in the vacuum consumable arc furnace melting station for furnace sealing and evacuation. S203, during the melting process, gas is injected into the gap between the melted consumable electrode and the crucible using a pressure control method. The melting voltage is 24-34V, the melting current is 8-16kA, and the arc stabilization current is 10-20A AC. S204, when the remaining weight of the consumable electrode is 70~250kg, feeding begins and gas is injected using a flow control method. After melting, cooling is still carried out by injecting gas. Then the consumable electrode is cooled normally and taken out of the furnace, finally obtaining a titanium alloy ingot.

3. The ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy according to claim 1, characterized in that, In S3, the forging process includes: after trimming the titanium alloy ingot, it is forged at a blanking temperature of 1080-1200℃, held for 90 minutes, and the deformation is ≥30%; then, a cyclic forging process of high-temperature forging + two-phase zone forging is performed, with the high-temperature forging temperature being 920-1000℃ and the deformation being ≥30%, and the two-phase zone forging temperature being 830-860℃ and the deformation being ≥20%; after the cyclic forging, it is drawn in multiple passes at a temperature of 820-870℃ to obtain the forged billet.

4. The ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy according to claim 1, characterized in that, In S3, the rolling process is as follows: multiple hot rolling passes are performed at 50~130℃ below the phase transformation point, with a deformation of 71%~88%, to obtain the hot-rolled billet.

5. The ultra-high strength and high plasticity Ti-Al-Mo-Zr-Sn-Cr-Fe titanium alloy according to claim 1, characterized in that, In S3, the ultra-high strength and high plasticity titanium alloy has a tensile strength of over 1500 MPa, an elongation of over 16%, and a reduction of area of ​​over 40%.

Citation Information

Patent Citations

  • A kind of nearly beta type high-strength high-toughness titanium alloy and its preparation method

    CN106507832B

  • High hardness titanium alloy and preparing method thereof

    CN108531774A

  • VAR smelting method for preparing large-size easy-segregation titanium alloy cast ingot in intensive cooling mode

    CN113186406A