Preparation method of graphene composite regenerated polyester staple fiber
By combining graphene-regenerated polyester staple fiber with graphene oxide and silver ions, the problem of traditional polyester fiber's inability to resist bacteria and mites is solved, achieving antibacterial and anti-mite effects and stability in the fiber, making it suitable for textiles and household products.
Patent Information
- Application Number
- CN202410215481.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-27
AI Technical Summary
Traditional polyester fibers cannot effectively kill bacteria and mites, and cannot meet the health needs of people with allergies or sensitive skin.
A method for preparing graphene-composite recycled polyester staple fiber is adopted, which combines graphene oxide with recycled polyester staple fiber, adds silver ions and polyvinyl alcohol, and utilizes the antibacterial properties of graphene oxide and the bactericidal effect of silver ions, combined with vacuum drying treatment to enhance the bonding force and stability of the fiber.
It achieves antibacterial and anti-mite effects on fibers, improves fiber durability and stability, conforms to the concept of sustainable development, and provides a healthy and safe living environment.
Abstract
Description
Technical Field
[0001] This application relates to the field of polyester fibers, and more specifically, to a graphene composite recycled polyester staple fiber and its preparation method. Background Technology
[0002] Polyester, scientifically known as polyester fiber, is a type of synthetic fiber and is a polymer compound obtained through polymerization.
[0003] Polyester exhibits diverse characteristics in its textile applications. Firstly, its fine fiber density allows for the creation of lightweight, breathable fabrics, ideal for summer clothing. Secondly, polyester's excellent dyeing properties enable a wide range of colors, allowing for various fabric production to meet the demands of fashion trends. Furthermore, polyester staple fibers can be spun purely or blended with other fibers. They can be blended with natural fibers such as cotton, linen, and wool, as well as with chemical staple fibers such as viscose, acetate, and polyacrylonitrile fibers, to produce a variety of textiles.
[0004] As living standards improve, people's demands for textiles are no longer limited to basic skin-friendliness and aesthetics; the antibacterial and anti-mite capabilities of textiles have also become an important factor for consumers. This is especially true for people with allergies or sensitive skin, as bacteria and mites on textiles can cause discomfort. Traditional polyester fibers cannot achieve the desired antibacterial and anti-mite effects, therefore, improvements to polyester fibers are needed to meet consumers' health needs. Summary of the Invention
[0005] In order to obtain a polyester fiber with antibacterial and anti-mite capabilities, this application provides a method for preparing graphene composite recycled polyester staple fiber.
[0006] The method for preparing graphene composite recycled polyester staple fiber provided in this application adopts the following technical solution: A method for preparing graphene-composite recycled polyester staple fiber includes the following steps: S1. Disperse 1-5 parts by weight of graphene oxide in 30-50 parts by weight of deionized water to obtain a graphene oxide dispersion; weigh 10-30 parts by weight of hydroxypropyl methylcellulose and dissolve it in 50-80 parts by weight of deionized water, heat to 80-90℃ and stir until completely dissolved to obtain an aqueous solution of hydroxypropyl methylcellulose; combine the graphene oxide solution and the aqueous solution of hydroxypropyl methylcellulose and sonicate for 20-30 minutes to obtain a graphene oxide / hydroxypropyl methylcellulose dispersion. S2. At a constant temperature of 50-70℃, mix 15-25 parts by weight of graphene oxide / hydroxypropyl methylcellulose dispersion, 1-5 parts by weight of silver nitrate solution and 0.1-0.5 parts by weight of sodium hydroxide solution, stir for 10 min to obtain a mixture, add 0.1-0.3 parts by weight of sodium borohydride solution dropwise to the mixture and stir for 2 h, then sonicate for 20-30 min to obtain a composite hydrogel; S3. Immerse recycled polyester staple fibers in NaOH solution at a bath ratio of 1:(15-25) for 1-2 hours. After treatment, remove the fibers, wash them with distilled water, and dry them in an oven at 50-60℃. After drying, immerse 30-50 parts of recycled polyester staple fibers in 50-100 parts of composite hydrogel. Then place the composite hydrogel containing recycled polyester staple fibers in a vacuum dryer and dry it at -5℃ to 0℃ for 10-14 hours. After completion, remove the fibers to obtain graphene composite recycled polyester staple fibers.
[0007] By employing the above-mentioned technical solutions, graphene oxide exhibits excellent antibacterial properties, effectively inhibiting and killing various bacteria. Combining graphene oxide with recycled polyester staple fibers endows the fibers with antibacterial capabilities. Further enhancing the antibacterial effect by combining graphene oxide with silver ions. Low-temperature treatment in a vacuum dryer helps maintain the shape and dimensional stability of the fibers while promoting the uniform formation of hydrogel films on the fiber surface. This treatment method not only strengthens the bond between the fiber and the hydrogel but also improves the fiber's durability and stability, resulting in a longer service life in practical applications.
[0008] Optionally, the method for preparing the graphene oxide is as follows: Add 3-5 parts by weight of graphite powder, 30-50 parts by weight of sulfuric acid solution, and 1-3 parts by weight of sodium nitrate to a container. Stir thoroughly at 0-5℃, then add 8-10 parts by weight of potassium permanganate and stir for 20-40 minutes. Then raise the temperature to 20-30℃ and stir for 30-60 minutes. Raise the temperature to 35-40℃ and keep it at that temperature for 10-12 hours. Then lower the temperature to 0-5℃ and add 100-150 parts by weight of deionized water and 15-25 parts by weight of 30% hydrogen peroxide. Stir until the mixed solution turns brownish-yellow. Add 150-200 parts by weight of dilute hydrochloric acid and let it settle for 10-12 hours. After centrifugation, discard the supernatant. Freeze-dry the obtained solid precipitate at ≤-50℃ for 10-16 hours to obtain graphene oxide.
[0009] By employing the above-described technical solution, this method is carried out under low-temperature conditions. By controlling the gradual increase in temperature and the holding time, the graphite powder can be fully oxidized to obtain highly oxidized graphene oxide. The use of sulfuric acid solution and sodium nitrate ensures good dispersibility of the graphene during oxidation, preventing agglomeration. The addition of potassium permanganate and hydrogen peroxide further enhances the structural stability of the graphene oxide, making it more stable in subsequent applications. This method utilizes continuous heating and cooling steps, as well as purification methods such as centrifugation and freeze-drying, simplifying the operation process and facilitating large-scale production.
[0010] Optionally, the method for preparing the recycled polyester staple fiber is as follows: The recycled waste PET plastic is crushed and washed to obtain PET granules. The PET granules are dried, and additives are added to the PET granules and mixed evenly. After melting and mixing, the mixture is spun and then drawn, dried and shaped to obtain recycled polyester staple fiber.
[0011] By adopting the above technical solution, this method utilizes waste PET plastic as raw material, realizing the reuse of waste, reducing environmental pollution, and conforming to the concept of sustainable development. Through steps such as crushing, washing, and drying, waste PET plastic is efficiently converted into recycled polyester staple fiber, improving resource utilization. Through a series of spinning processes, such as drawing, drying, and setting, the quality and performance of recycled polyester staple fiber can be guaranteed, making it reach or approach the standards of virgin polyester staple fiber.
[0012] Optionally, the additives include 40-60% zinc oxide powder and 40-60% polyester chain extender.
[0013] By adopting the above technical solutions, zinc oxide powder can impart antibacterial and anti-mite properties to fibers, increasing the added value of recycled polyester staple fiber. Simultaneously, polyester chain extenders help improve the strength, toughness, and abrasion resistance of the fibers, making their properties closer to those of virgin polyester staple fiber. Polyester chain extenders can increase the cross-linking between fiber molecules, improving their thermal stability, chemical stability, and light stability, thus giving recycled polyester staple fiber better durability in practical applications. Adding an appropriate amount of polyester chain extender can improve the spinning performance of the fiber, lower the spinning temperature, reduce fiber breakage and fuzzing during the spinning process, and improve spinning efficiency and product quality.
[0014] Optionally, in step S3, 20-40 parts by weight of polyvinyl alcohol are added to the composite hydrogel before vacuum drying, the temperature is raised to 80-90°C and stirred evenly.
[0015] By adopting the above technical solution, polyvinyl alcohol exhibits excellent adhesion and film-forming properties, allowing it to better integrate with components in the composite hydrogel and further enhance the bonding force between the fiber and the hydrogel. The addition of polyvinyl alcohol can form a protective film on the fiber surface, improving the fiber's flexibility and tensile strength, thus giving it better durability and stability in practical applications.
[0016] Optionally, the concentration of the NaOH solution in step S3 is 8-12 g·L.
[0017] Optionally, the concentration of the silver nitrate solution in step S2 is 0.1-0.3 mol / L.
[0018] Optionally, the concentration of sodium borohydride solution in step S2 is 0.05-0.2 mol / L.
[0019] By employing the above-mentioned technical solution, treatment in a strongly alkaline environment can alter the polarity and crystallinity of the fiber surface, thereby enhancing the adsorption capacity of the polyester fiber surface. Appropriate concentrations of silver nitrate and sodium borohydride can optimize the reaction rate, resulting in more uniform and rapid formation of the composite hydrogel and improved production efficiency.
[0020] In summary, this application has the following beneficial effects: 1. This application utilizes a composite of graphene oxide with silver ions and polyester fibers. Silver ions possess a strong bactericidal effect against various bacteria and microorganisms. They can bind to the DNA of microorganisms, preventing their replication and thus achieving a bactericidal effect. Secondly, graphene oxide exhibits excellent antibacterial properties. It can disrupt the cell membrane of bacteria, leading to bacterial death. When silver ions and graphene oxide combine, they work synergistically to produce a stronger antibacterial and antifungal effect. This composite material can not only kill or inhibit the growth of bacteria, mold, and other microorganisms, but also effectively remove mites. This is of great significance for products in the textile and household goods industries, providing people with a healthier and safer living environment.
[0021] 2. In this application, polyvinyl alcohol is preferably used due to its excellent adhesion and film-forming properties. It can better combine with the components in the composite hydrogel, further enhancing the bonding force between the fiber and the hydrogel. The addition of polyvinyl alcohol can form a protective film on the fiber surface, improving the fiber's flexibility and tensile strength, thus giving it better durability and stability in practical applications.
[0022] 3. This application preferably utilizes waste PET plastic as raw material, thereby achieving waste reuse, reducing environmental pollution, and conforming to the concept of sustainable development. Detailed Implementation
[0023] The present application will be further described in detail below with reference to the embodiments.
[0024] Preparation example of graphene oxide Preparation Example 1 4 kg of graphite powder, 40 kg of 0.5 mol / L sulfuric acid solution, and 2 kg of sodium nitrate were added to a container. After thorough mixing at 3°C, 9 kg of potassium permanganate was added and stirred for 30 min. The temperature was then raised to 25°C and stirred for 40 min. The temperature was then raised to 38°C and kept at that temperature for 11 h. The temperature was then lowered to 3°C and 120 kg of deionized water and 20 kg of 30% hydrogen peroxide were added dropwise. The mixture was stirred until the solution turned brownish-yellow. 180 kg of 0.2 mol / kg dilute hydrochloric acid was added and allowed to settle for 11 h. After centrifugation, the supernatant was discarded. The resulting solid precipitate was freeze-dried at -50°C for 14 h to obtain graphene oxide.
[0025] Example of preparation of recycled polyester staple fiber Preparation Example 2 The recycled waste PET plastic is crushed and washed to obtain PET granules. 50 kg of PET granules are dried, and 10 kg of zinc oxide powder and 10 kg of polyester chain extender are added to the PET granules and mixed evenly. The mixture is then heated to 250°C to melt, and then spun through a double roller mill. After stretching, drying and shaping, 50 mm long recycled polyester staple fibers are obtained.
[0026] Preparation Example 3 The recycled waste PET plastic is crushed and washed to obtain PET granules. 50 kg of PET granules are dried, and 8 kg of zinc oxide powder and 12 kg of polyester chain extender are added to the PET granules and mixed evenly. The mixture is then heated to 250°C to melt, and then spun through a double roller mill. After stretching, drying and setting, 50 mm long recycled polyester staple fibers are obtained.
[0027] Preparation Example 4 The recycled waste PET plastic is crushed and washed to obtain PET granules. 50 kg of PET granules are dried, and 12 kg of zinc oxide powder and 8 kg of polyester chain extender are added to the PET granules and mixed evenly. The mixture is then heated to 250°C to melt, and then spun through a double roller mill. After stretching, drying and setting, 50 mm long recycled polyester staple fibers are obtained. Example
[0028] Example 1 A method for preparing graphene-composite recycled polyester staple fiber: S1. Disperse 3 kg of graphene oxide in 40 kg of deionized water to obtain a graphene oxide dispersion; weigh 20 kg of hydroxypropyl methylcellulose and dissolve it in 60 kg of deionized water, heat to 85 °C and stir until completely dissolved to obtain a hydroxypropyl methylcellulose aqueous solution; combine the graphene oxide solution and the hydroxypropyl methylcellulose aqueous solution and sonicate for 25 min to obtain a graphene oxide / hydroxypropyl methylcellulose dispersion. S2. At a constant temperature of 60℃, 20 kg of graphene oxide / hydroxypropyl methylcellulose dispersion, 3 kg of silver nitrate solution, and 0.3 kg of sodium hydroxide solution were mixed. The concentration of silver nitrate solution was 0.2 mol / L. The mixture was stirred for 10 min to obtain a mixed solution. 0.2 kg of 0.1 mol / L sodium borohydride solution was added dropwise to the mixed solution and the mixture was stirred and reacted for 2 h. The mixture was then sonicated for 25 min to obtain a composite hydrogel. S3. The recycled polyester staple fiber was immersed in NaOH solution with a concentration of 10 g·L and a bath ratio of 1:20. After treatment for 1.5 h, it was taken out and washed with distilled water and placed in an oven at 55 ℃ to dry. After drying, 4 kg of recycled polyester staple fiber was immersed in 8 kg of composite hydrogel. The composite hydrogel containing recycled polyester staple fiber was then placed in a vacuum dryer and placed at -3 ℃ for 12 h. After completion, it was taken out to obtain graphene composite recycled polyester staple fiber.
[0029] In this study, graphene oxide was prepared in Preparation Example 1, and recycled polyester staple fiber was prepared in Preparation Example 2.
[0030] Example 2 A method for preparing graphene composite recycled polyester staple fiber differs from Example 1 in that: in step S3, 30 kg of polyvinyl alcohol is added to the composite hydrogel before vacuum drying, the temperature is raised to 85°C, and the mixture is stirred until homogeneous. Example 3 A method for preparing graphene composite recycled polyester staple fiber differs from Example 1 in that the concentration of NaOH solution in step S3 is 8 g·L.
[0031] Example 4 A method for preparing graphene composite recycled polyester staple fiber differs from Example 1 in that the concentration of NaOH solution in step S3 is 12 g·L.
[0032] Example 5 A method for preparing graphene composite recycled polyester staple fiber differs from Example 1 in that the concentration of silver nitrate solution in step S2 is 0.1 mol / L.
[0033] Example 6 A method for preparing graphene composite recycled polyester staple fiber differs from Example 1 in that the concentration of silver nitrate solution in step S2 is 0.3 mol / L.
[0034] Example 7 A method for preparing graphene composite recycled polyester staple fiber differs from Example 1 in that the concentration of sodium borohydride solution in step S2 is 0.05 mol / L.
[0035] Example 8 A method for preparing graphene composite recycled polyester staple fiber differs from Example 1 in that the concentration of sodium borohydride solution in step S2 is 0.2 mol / L.
[0036] Example 9 A method for preparing graphene composite recycled polyester staple fiber differs from Example 1 in that the recycled polyester staple fiber is prepared by Example 3.
[0037] Example 10 A method for preparing graphene composite recycled polyester staple fiber differs from Example 1 in that the recycled polyester staple fiber is prepared by Example 4.
[0038] Comparative Example Comparative Example 1 A method for preparing graphene-composite recycled polyester staple fiber: S1. Disperse 3 kg of graphene in 40 kg of deionized water to obtain a graphene dispersion; weigh 20 kg of hydroxypropyl methylcellulose and dissolve it in 60 kg of deionized water, heat to 85 °C and stir until completely dissolved to obtain a hydroxypropyl methylcellulose aqueous solution; combine the graphene solution and the hydroxypropyl methylcellulose aqueous solution and sonicate for 25 min to obtain a graphene / hydroxypropyl methylcellulose dispersion. S2. At a constant temperature of 60℃, 20 kg of graphene / hydroxypropyl methylcellulose dispersion, 3 kg of silver nitrate solution, and 0.3 kg of sodium hydroxide solution were mixed. The concentration of silver nitrate solution was 0.2 mol / L. The mixture was stirred for 10 min to obtain a mixture. 0.2 kg of 0.1 mol / L sodium borohydride solution was added dropwise to the mixture and the mixture was stirred and reacted for 2 h. The mixture was then sonicated for 25 min to obtain a composite hydrogel. S3. The recycled polyester staple fiber was immersed in NaOH solution with a concentration of 10 g·L and a bath ratio of 1:20. After treatment for 1.5 h, it was taken out and washed with distilled water and placed in an oven at 55 ℃ to dry. After drying, 4 kg of recycled polyester staple fiber was immersed in 8 kg of composite hydrogel. The composite hydrogel containing recycled polyester staple fiber was then placed in a vacuum dryer and placed at -3 ℃ for 12 h. After completion, it was taken out to obtain graphene composite recycled polyester staple fiber.
[0039] The recycled polyester staple fiber was prepared in Preparation Example 2.
[0040] Comparative Example 2 A method for preparing graphene-composite polyester staple fiber: S1. Disperse 3 kg of graphene oxide in 40 kg of deionized water to obtain a graphene oxide dispersion; weigh 20 kg of hydroxypropyl methylcellulose and dissolve it in 60 kg of deionized water, heat to 85 °C and stir until completely dissolved to obtain a hydroxypropyl methylcellulose aqueous solution; combine the graphene oxide solution and the hydroxypropyl methylcellulose aqueous solution and sonicate for 25 min to obtain a graphene oxide / hydroxypropyl methylcellulose dispersion. S2. At a constant temperature of 60℃, 20 kg of graphene oxide / hydroxypropyl methylcellulose dispersion, 3 kg of silver nitrate solution, and 0.3 kg of sodium hydroxide solution were mixed. The concentration of silver nitrate solution was 0.2 mol / L. The mixture was stirred for 10 min to obtain a mixed solution. 0.2 kg of 0.1 mol / L sodium borohydride solution was added dropwise to the mixed solution and the mixture was stirred and reacted for 2 h. The mixture was then sonicated for 25 min to obtain a composite hydrogel. S3. The polyester staple fiber was immersed in NaOH solution with a concentration of 10 g·L and a bath ratio of 1:20. After treatment for 1.5 h, it was taken out and washed with distilled water and placed in an oven at 55 ℃ to dry. After drying, 4 kg of polyester staple fiber was immersed in 8 kg of composite hydrogel. The composite hydrogel containing polyester staple fiber was then placed in a vacuum dryer and placed at -3 ℃ for 12 h. After completion, it was taken out to obtain graphene composite polyester staple fiber.
[0041] In this study, graphene oxide was prepared by Preparation Example 1, and polyester staple fiber was obtained commercially available.
[0042] Comparative Example 3 A method for preparing graphene-composite recycled polyester staple fiber: S1. Disperse 3 kg of graphene oxide in 40 kg of deionized water to obtain a graphene oxide dispersion; weigh 20 kg of hydroxypropyl methylcellulose and dissolve it in 60 kg of deionized water, heat to 85 °C and stir until completely dissolved to obtain a hydroxypropyl methylcellulose aqueous solution; combine the graphene oxide solution and the hydroxypropyl methylcellulose aqueous solution and sonicate for 25 min to obtain a graphene oxide / hydroxypropyl methylcellulose dispersion. S2. Recycled polyester staple fiber is immersed in NaOH solution with a concentration of 10 g·L and a bath ratio of 1:20. After treatment for 1.5 h, it is taken out and washed with distilled water, and placed in an oven at 55 ℃ to dry. After drying, 4 kg of recycled polyester staple fiber is immersed in 8 kg of graphene oxide / hydroxypropyl methylcellulose dispersion. Then, the graphene oxide / hydroxypropyl methylcellulose dispersion containing recycled polyester staple fiber is placed in a vacuum dryer and placed at -3 ℃ for 12 h. After completion, it is taken out to obtain graphene composite recycled polyester staple fiber.
[0043] In this study, graphene oxide was prepared in Preparation Example 1, and recycled polyester staple fiber was prepared in Preparation Example 2.
[0044] Performance testing Detection methods Staphylococcus aureus and Escherichia coli were used to evaluate the antibacterial properties of the samples before and after modification. The specific steps were as follows: 0.1 g of the sample was ultrasonically dispersed in 10 mL of phosphate-buffered saline (PBS), and then 100 μL of bacterial suspension was added. After a 30-minute contact time, the bacterial suspension sample was removed, and 4.5 mL of PBS / Na₂S₂O₃ solution was added to neutralize any residual active chlorine in the suspension. The above solution (100 μL) was continuously diluted multiple times with PBS buffer, and the diluted solution was dropped onto the surface of agar medium. After 24 hours of incubation at 37°C, the bacterial colonies on the medium were determined to calculate the antibacterial efficiency.
[0045] Mites were cultured under laboratory conditions to obtain a sufficient number of mites. The test samples were placed in petri dishes containing 500 ± 10 mites, ensuring uniform mite distribution. The petri dishes were then incubated in a temperature- and humidity-controlled incubator for 24 hours, after which the mite mortality rate was determined.
[0046] The tensile strength of graphene-composite recycled polyester staple fiber was determined using a universal tensile testing machine.
[0047] Table 1 Statistical analysis of experimental results Antibacterial rate / % Mite removal rate / % Tensile strength cN / dtex Example 1 98.8 89.8 5.87 Example 2 99.1 90.3 5.95 Example 3 97.6 88.8 5.71 Example 4 96.5 86.4 5.33 Example 5 97.7 86.2 5.15 Example 6 98.1 87.6 5.45 Example 7 97.4 88.1 5.65 Example 8 96.8 88.6 4.98 Example 9 98.2 86.9 5.36 Example 10 97.3 88.6 5.47 Comparative Example 1 73.4 65.7 4.88 Comparative Example 2 95.3 81.2 6.03 Comparative Example 3 75.6 56.5 4.65 As can be seen from Example 1 and Comparative Example 1, and Table 1, the antibacterial and anti-mite performance of graphene oxide composite with polyester fiber is better. Graphene oxide has excellent antibacterial properties and can effectively inhibit and kill a variety of bacteria.
[0048] As can be seen from Example 1 and Comparative Example 2, and Table 1, a series of spinning processes, such as drawing, drying, and setting, can ensure the quality and performance of recycled polyester staple fiber, making it reach or approach the standard of virgin polyester staple fiber.
[0049] As can be seen from Example 1 and Comparative Example 3, and Table 1, when silver ions combine with graphene oxide, the antibacterial properties of graphene oxide can be further enhanced, and the antibacterial effect of silver ions can also be improved.
[0050] As can be seen from Examples 1-2 and Table 1, polyvinyl alcohol has good adhesion and film-forming properties, and it can better combine with the components in the composite hydrogel, further enhancing the bonding force between the fiber and the hydrogel.
[0051] As can be seen from Examples 1 and 3-8, and Table 1, treatment in a strongly alkaline environment can alter the polarity and crystallinity of the fiber surface, thereby improving the adsorption capacity of the polyester fiber surface. Appropriate concentrations of silver nitrate and sodium borohydride can optimize the reaction rate, resulting in a more uniform and rapid formation of the composite hydrogel, thus improving production efficiency. Example 1 represents the optimal solution of this application.
[0052] As can be seen from Examples 1 and 9-10, and Table 1, zinc oxide powder can impart antibacterial and anti-mite properties to fibers, increasing the added value of recycled polyester staple fiber. Simultaneously, polyester chain extenders help improve the strength, toughness, and abrasion resistance of the fiber, making its properties closer to those of virgin polyester staple fiber. By adjusting the amount of additives, graphene composite recycled polyester staple fiber with even better performance can be obtained.
[0053] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A method for preparing graphene-composite recycled polyester staple fiber, characterized in that, Includes the following steps: S1. Disperse 1-5 parts by weight of graphene oxide in 30-50 parts by weight of deionized water to obtain a graphene oxide dispersion; weigh 10-30 parts by weight of hydroxypropyl methylcellulose and dissolve it in 50-80 parts by weight of deionized water, heat to 80-90℃ and stir until completely dissolved to obtain a hydroxypropyl methylcellulose aqueous solution; mix the graphene oxide solution and the hydroxypropyl methylcellulose aqueous solution and sonicate for 20-30 minutes to obtain a graphene oxide / hydroxypropyl methylcellulose dispersion; S2. At a constant temperature of 50-70℃, mix 15-25 parts by weight of graphene oxide / hydroxypropyl methylcellulose dispersion, 1-5 parts by weight of silver nitrate solution and 0.1-0.5 parts by weight of sodium hydroxide solution, stir for 10 min to obtain a mixture, add 0.1-0.3 parts by weight of sodium borohydride solution dropwise to the mixture and stir for 2 h, then sonicate for 20-30 min to obtain a composite hydrogel; S3. Immerse recycled polyester staple fibers in NaOH solution at a bath ratio of 1:(15-25) for 1-2 hours. After treatment, remove the fibers, wash them with distilled water, and dry them in an oven at 50-60℃. After drying, immerse 30-50 parts of recycled polyester staple fibers in 50-100 parts of composite hydrogel. Add 20-40 parts by weight of polyvinyl alcohol to the composite hydrogel, heat it to 80-90℃ and stir it evenly. Then place the composite hydrogel containing recycled polyester staple fibers in a vacuum dryer and place it at -5℃-0℃ for 10-14 hours. After completion, remove the fibers to obtain graphene composite recycled polyester staple fibers. The concentration of the NaOH solution in step S3 is 8-12 g·L⁻¹.
2. The method for preparing graphene composite recycled polyester staple fiber according to claim 1, characterized in that: The preparation method of the graphene oxide is as follows: Add 3-5 parts by weight of graphite powder, 30-50 parts by weight of sulfuric acid solution, and 1-3 parts by weight of sodium nitrate to a container. Stir thoroughly at 0-5℃, then add 8-10 parts by weight of potassium permanganate and stir for 20-40 minutes. Then raise the temperature to 20-30℃ and stir for 30-60 minutes. Raise the temperature to 35-40℃ and keep it at that temperature for 10-12 hours. Then lower the temperature to 0-5℃ and add 100-150 parts by weight of deionized water and 15-25 parts by weight of 30% hydrogen peroxide. Stir until the mixed solution turns brownish-yellow. Add 150-200 parts by weight of dilute hydrochloric acid and let it settle for 10-12 hours. After centrifugation, discard the supernatant. Freeze-dry the obtained solid precipitate at ≤-50℃ for 10-16 hours to obtain graphene oxide.
3. The method for preparing graphene composite recycled polyester staple fiber according to claim 1, characterized in that: In step S2, the concentration of the silver nitrate solution is 0.1-0.3 mol / L.
4. The method for preparing graphene composite recycled polyester staple fiber according to claim 1, characterized in that: In step S2, the concentration of sodium borohydride solution is 0.05-0.2 mol / L.
Citation Information
Patent Citations
Regenerated polyester staple fiber and preparation method thereof
CN106835310A
Polyester fabric with antistatic and antibacterial functions and preparation method of polyester fabric
CN110438800A
Composite non-woven fabric with high water absorption and high strength
CN111016344A
Modified graphene loaded nano-silver / polyvinyl alcohol antibacterial hydrogel and preparation method thereof
CN113637183A
Cellulose / acrylamide photothermal conversion hydrogel as well as preparation method and application thereof
CN117586454A