A carbon fiber surface modification method, modified carbon fiber and carbon fiber reinforced resin matrix composite
By forming PEI nanoparticles on the surface of carbon fibers through a low-temperature evaporation-induced method, the problems of complex and costly surface modification of existing carbon fibers are solved, the interfacial bonding performance between carbon fibers and resins is improved, and it is suitable for industrial production.
Patent Information
- Application Number
- CN202410236200.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-01
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-01
AI Technical Summary
Existing carbon fiber surface modification methods are complex, costly, and unsafe, making them difficult to apply industrially, and they also have poor interfacial bonding performance.
Low-temperature evaporation was used to induce polyetherimide (PEI) nanoparticles to form a hemispherical structure on the carbon fiber surface, which improved the surface roughness and activity, and enhanced the interfacial bonding with the resin.
This method achieves simple, safe, and low-cost surface modification of carbon fibers, enhances the interfacial bonding performance between carbon fibers and resins, and is suitable for industrial production.
Smart Images

Figure CN118029160B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon fiber surface modification technology, and in particular to a method for carbon fiber surface modification, modified carbon fibers, and carbon fiber reinforced resin matrix composites. Background Technology
[0002] The information disclosed in the background section of this invention is intended only to enhance the understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.
[0003] Carbon fiber reinforced resin matrix composites (CFRPs) are widely used in aerospace, transportation, and civilian fields due to their excellent mechanical properties and low density. In these composites, the carbon fiber reinforcement is the main load-bearing component, the resin matrix is the medium for load transfer, and the interface ensures the continuous propagation of load between the reinforcement and the matrix. Therefore, the interface is often a key factor determining the mechanical properties of composites. Thus, surface modification of carbon fibers can improve the interfacial bonding and mechanical properties of composites.
[0004] In recent years, in addition to wet and dry modification of carbon fibers, "multi-scale" modification has attracted increasing attention from researchers. This involves grafting nanomaterials onto the surface of carbon fibers to increase surface roughness and enhance surface activity, which is beneficial for resin wetting and forming mechanical interlock with the resin.
[0005] Patent CN 104499270 B (authorization announcement date: 2016.07.06) discloses a method for modifying carbon fiber surface with nano-silica. This method involves alkynylating the carbon fiber surface and then grafting azidated nano-silica onto it via a chemical reaction, thereby increasing the wettability and roughness of the carbon fiber surface. However, this method is complex and cumbersome, has a long preparation process, and involves high risks related to raw materials and the preparation process, resulting in high costs and making it difficult to apply industrially.
[0006] Patent CN 107407042 B (authorization announcement date: July 21, 2020) discloses a fiber sizing system containing nanoparticles for carbon fibers. It uses an aqueous emulsion containing silica nanoparticles as a sizing agent to modify the carbon fibers, thereby improving the adhesion and wetting properties between the carbon fibers and the resin. However, this sizing agent is not environmentally friendly, has poor stability, and its preparation process is complex, making industrial production difficult.
[0007] Therefore, how to provide a simple, low-cost, and safe method for grafting nanomaterials onto the surface of carbon fibers is an urgent problem to be solved. Summary of the Invention
[0008] In view of this, the present invention provides a method for modifying the surface of carbon fibers, modified carbon fibers, and carbon fiber reinforced resin matrix composites. The present invention improves the surface roughness, surface wettability, and activity of carbon fibers by inducing polyetherimide (PEI) nanoparticles through low-temperature evaporation on the surface of carbon fibers, which is beneficial to resin wetting and forming mechanical interlock with the resin, thereby improving the interfacial bonding between carbon fibers and resin. The surface modification method is simple, low-cost, and highly safe.
[0009] In a first aspect, the present invention provides a method for modifying the surface of carbon fibers, comprising the following steps:
[0010] The desized carbon fiber was placed in a polyetherimide solution and sonicated at -5 to 3°C for 10 to 30 minutes, then kept at the temperature and allowed to stand for 20 to 30 hours. After standing, it was taken out and evaporated at 10 to 30°C.
[0011] Preferably, the desized carbon fiber is prepared by heating the carbon fiber to 400-500°C in an inert gas atmosphere, holding it at that temperature for 1-2 hours, cooling it to room temperature, washing it, and drying it to obtain the carbon fiber.
[0012] Furthermore, the inert gas includes one or both of nitrogen or argon; the solvent used in the washing step is water or ethanol.
[0013] Preferably, before placing the desized carbon fiber in the polyetherimide solution, the desized carbon fiber is pre-impregnated with the solvent of the polyetherimide solution for 10 to 30 minutes.
[0014] Preferably, the ratio of the desized carbon fiber to the polyetherimide solution is 1g:300-700mL.
[0015] Preferably, the mass concentration of the polyetherimide solution is 0.1 to 0.6 wt%.
[0016] Preferably, the solvent of the polyetherimide solution is selected from one or more of N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), or N,N-dimethylacetamide (DMAc).
[0017] Furthermore, the polyetherimide solution is prepared by placing polyetherimide in a solvent and stirring to dissolve it at 60–80°C for 1–4 hours.
[0018] Secondly, the present invention provides a modified carbon fiber prepared by the above-mentioned carbon fiber surface modification method.
[0019] Thirdly, the present invention provides a carbon fiber reinforced resin matrix composite material comprising the above-mentioned modified carbon fiber.
[0020] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0021] (1) The present invention provides a carbon fiber surface modification method, which obtains uniformly distributed hemispherical PEI nanoparticles on the carbon fiber surface by low temperature evaporation induction, which can increase the surface roughness and surface activity of carbon fiber, which is beneficial to resin wetting and forming mechanical interlock with resin, thereby improving the interfacial bonding between carbon fiber and resin.
[0022] (2) The carbon fiber surface modification method provided by the present invention is simple, easy to operate, and low in cost. Moreover, the operation is carried out at a low temperature, which makes it safe and suitable for industrial production. Attached Figure Description
[0023] The accompanying drawings, which form part of this specification, are used to provide a further understanding of the invention. The illustrative embodiments and descriptions of the invention are used to explain the invention and do not constitute an undue limitation thereof. Obviously, those skilled in the art can obtain other drawings based on these drawings without any inventive effort.
[0024] Figure 1 These are scanning electron microscope images of the surface of the modified carbon fiber of Embodiment 1 of the present invention;
[0025] Figure 2 These are scanning electron microscope images of the surface of the modified carbon fiber in Example 2 of this invention;
[0026] Figure 3 These are scanning electron microscope images of the surface of the modified carbon fiber of Comparative Example 1 of this invention;
[0027] Figure 4 These are scanning electron microscope images of the surface of the modified carbon fiber of Comparative Example 2 of this invention;
[0028] Figure 5 These are interlaminar shear strength diagrams of composite materials prepared from modified carbon fibers and untreated carbon fibers in Examples 1 and 2 of this invention. Detailed Implementation
[0029] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0030] This invention provides a method for modifying the surface of carbon fibers, comprising the following steps:
[0031] The desized carbon fiber was placed in a polyetherimide solution and sonicated at -5 to 3°C for 10 to 30 minutes, then kept at the temperature and allowed to stand for 20 to 30 hours. After standing, it was taken out and evaporated at 10 to 30°C.
[0032] This invention utilizes polyetherimide (PEI) nanoparticles to modify the surface of carbon fibers. PEI is an amorphous thermoplastic whose molecular chain contains benzene rings and semi-trapezoidal imide bonds, giving it excellent heat resistance. Furthermore, the benzene rings and imide bonds in PEI can chemically bond with resins, thereby strengthening the interfacial bonding. It can withstand processing temperatures above 350℃ and also exhibits excellent chemical resistance and good mechanical properties. Combining PEI nanoparticles with carbon fibers improves the surface roughness and wettability of the carbon fibers, thereby enhancing the interfacial bonding performance between the carbon fibers and the resin.
[0033] This invention employs a low-temperature evaporation-induced method. The evaporation process is dynamic; as the solvent decreases, the solute concentration increases. At low temperatures, the evaporation rate is very slow, and the PEI chains shrink from a long-chain state to a granular state under the influence of surface tension, ultimately forming hemispherical nanoparticles. Temperature plays a crucial role in the surface modification process. If the temperature is too high, PEI will struggle to form nanoparticles on the carbon fiber surface, thus failing to fully realize its role in promoting the bonding between carbon fibers and resin.
[0034] In the carbon fiber production process, carbon fibers need to be sized to reduce surface friction and prevent fuzz formation during transportation. However, commercial sizing agents are not very effective in improving the interfacial properties of composite materials. Therefore, it is necessary to remove the commercial sizing agents used in the carbon fiber production process (i.e., desizing). In this invention, the desizing carbon fiber is prepared by heating the carbon fiber to 400-500°C in an inert gas atmosphere, holding it at that temperature for 1-2 hours, cooling it to room temperature, washing it, and drying it.
[0035] In the preparation of desized carbon fiber, the inert gas includes one or both of nitrogen or argon, and the solvent used in the washing step is water or ethanol to remove impurities from the surface of the carbon fiber.
[0036] In this invention, before placing the desized carbon fiber in the polyetherimide solution, the desized carbon fiber is pre-impregnated with the solvent of the polyetherimide solution for 10–30 minutes. This step is to improve the wetting rate of the desized carbon fiber in the polyetherimide solution.
[0037] In this invention, in order to ensure that the polyetherimide can uniformly impregnate the desized carbon fiber, the ratio of the amount of desized carbon fiber to the polyetherimide solution is 1g:300-700mL.
[0038] In this invention, the mass concentration of the polyetherimide solution is 0.1–0.6 wt%. If the concentration is too high, the PEI nanoparticles will aggregate, which is detrimental to their bonding with the resin.
[0039] The solvent for the polyetherimide solution described in this invention is selected from one or more of N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), or N,N-dimethylacetamide (DMAc). These solvents exhibit good solubility for PEI, have high boiling points, are not easily volatile, and do not solidify at the operating temperature.
[0040] To obtain a well-soluble polyetherimide solution, the polyetherimide was placed in the above solvent and stirred at 60–80°C for 1–4 hours to dissolve.
[0041] The present invention also provides a modified carbon fiber, which is prepared by the above-described carbon fiber surface modification method. The prepared modified carbon fiber has PEI nanoparticles with a hemispherical structure uniformly distributed on its surface.
[0042] This invention also provides a carbon fiber reinforced resin-based composite material comprising the aforementioned modified carbon fibers. This invention does not impose any particular limitation on the type of resin; it can be either a thermosetting resin or a thermoplastic resin. For example, it can be selected from epoxy resin, phenolic resin, polyimide resin, polypropylene resin, polyamide resin, polystyrene resin, etc.
[0043] The technical solution of the present invention will be further described below with reference to specific embodiments.
[0044] Example 1
[0045] This embodiment provides a method for inducing PEI nanoparticles by low-temperature evaporation on the surface of carbon fibers.
[0046] Step 1: Place the carbon fiber into a tube furnace and heat it to 450℃ for 1.5 hours in a nitrogen atmosphere to remove the sizing agent from the surface of the carbon fiber. After cooling to room temperature, take it out and wash it several times with deionized water. Then put it into an oven to dry and obtain desized carbon fiber.
[0047] Step 2: Place 1g of the desized carbon fiber obtained in Step 1 into N-methylpyrrolidone for 15 minutes.
[0048] Step 3: Dissolve PEI in N-methylpyrrolidone at 70℃ and stir for 2 hours, controlling the mass fraction of PEI in N-methylpyrrolidone to be 0.2wt%.
[0049] Step 4: Place the carbon fiber obtained in Step 2 in 500 mL of the PEI solution obtained in Step 3 in an ice bath (0℃) and sonicate for 20 min, then let it stand in an ice bath (0℃) for 24 h.
[0050] Step 5: Evaporate the carbon fiber obtained in Step 4 at 20°C until the carbon fiber is dry to obtain modified carbon fiber.
[0051] The surface scanning electron microscope image of the modified carbon fiber prepared in this embodiment is shown below. Figure 1 As shown, PEI nanoparticles are uniformly loaded onto the carbon fiber surface, increasing the surface roughness. The PEI nanoparticles exhibit a hemispherical structure on the carbon fiber surface, resulting in a large specific surface area.
[0052] Example 2
[0053] This embodiment provides a method for inducing PEI nanoparticles by low-temperature evaporation on the surface of carbon fibers.
[0054] Step 1: Place the carbon fiber into a tube furnace and heat it to 450℃ for 1.5 hours in a nitrogen atmosphere to remove the sizing agent from the surface of the carbon fiber. After cooling to room temperature, take it out and wash it several times with deionized water. Then put it into an oven to dry and obtain desized carbon fiber.
[0055] Step 2: Place 1g of the desized carbon fiber obtained in Step 1 into N-methylpyrrolidone for 15 minutes.
[0056] Step 3: Dissolve PEI in N-methylpyrrolidone at 70°C and stir for 2 hours to make the mass fraction of PEI in the N-methylpyrrolidone obtained in Step 3 0.3wt%.
[0057] Step 4: Place the carbon fiber obtained in Step 2 in 500 mL of the PEI solution obtained in Step 3 in an ice bath (0℃) and sonicate for 20 min, then let it stand in an ice bath (0℃) for 24 h.
[0058] Step 5: Evaporate the carbon fiber obtained in Step 4 at 20°C until the carbon fiber is dry to obtain modified carbon fiber.
[0059] The surface scanning electron microscope image of the modified carbon fiber prepared in this embodiment is shown below. Figure 2 As shown, PEI nanoparticles are uniformly loaded on the surface of the carbon fiber, which increases the roughness of the carbon fiber surface; the PEI nanoparticles have a hemispherical structure on the carbon fiber surface and have a large specific surface area.
[0060] Example 3
[0061] Step 1: Place the carbon fiber into a tube furnace and heat it to 450℃ for 1.5 hours in a nitrogen atmosphere to remove the sizing agent from the surface of the carbon fiber. After cooling to room temperature, take it out and wash it several times with deionized water. Then put it into an oven to dry and obtain desized carbon fiber.
[0062] Step 2: Place 1g of the desized carbon fiber obtained in Step 1 into N,N-dimethylformamide for 15 minutes.
[0063] Step 3: Dissolve PEI in N,N-dimethylformamide at 70℃ and stir for 2 hours to make the mass fraction of PEI in N,N-dimethylformamide 0.4wt%.
[0064] Step 4: Place the carbon fiber obtained in Step 2 in 500 mL of the PEI solution obtained in Step 3 in an ice bath (0℃) and sonicate for 20 min, then let it stand in an ice bath (0℃) for 24 h.
[0065] Step 5: Evaporate the carbon fiber obtained in Step 4 at 20°C until the carbon fiber is dry to obtain modified carbon fiber.
[0066] Example 4
[0067] Step 1: Place the carbon fiber into a tube furnace and heat it to 450℃ for 1.5 hours in a nitrogen atmosphere to remove the sizing agent from the surface of the carbon fiber. After cooling to room temperature, take it out and wash it several times with deionized water. Then put it into an oven to dry and obtain desized carbon fiber.
[0068] Step 2: Place 1g of the desized carbon fiber obtained in Step 1 into N-methylpyrrolidone for 15 minutes.
[0069] Step 3: Dissolve PEI in N-methylpyrrolidone in a 70℃ oil bath and stir for 2 hours to make the mass fraction of PEI in N-methylpyrrolidone 0.5wt%.
[0070] Step 4: Place the carbon fiber obtained in Step 2 in 500 mL of the PEI solution obtained in Step 3 in an ice bath (0℃) and sonicate for 20 min, then let it stand in an ice bath (0℃) for 24 h.
[0071] Step 5: Evaporate the carbon fiber obtained in Step 4 at 20°C until the carbon fiber is dry to obtain modified carbon fiber.
[0072] Comparative Example 1
[0073] Compared with Example 1, the difference is that step five of this comparative example is as follows: the carbon fiber obtained in step four is evaporated at 40°C until the carbon fiber is dry to obtain modified carbon fiber.
[0074] The surface scanning electron microscope image of the modified carbon fiber in this comparative example is shown below. Figure 3 As shown, it can be seen that there are unevenly sized protrusions on the surface of the carbon fiber. The particle size of the protrusions is very small, and there are no hemispherical nanoparticles with larger diameters, resulting in low roughness.
[0075] Comparative Example 2
[0076] Compared with Example 1, the difference is that step five of this comparative example is as follows: the carbon fiber obtained in step four is evaporated at 80°C until the carbon fiber is dry to obtain modified carbon fiber.
[0077] The surface scanning electron microscope image of the modified carbon fiber in this comparative example is shown below. Figure 4 As shown, the carbon fiber surface has a high degree of smoothness, and no nanoparticle formation was observed.
[0078] Test case
[0079] Carbon fiber reinforced polypropylene composites were prepared using untreated carbon fibers, Comparative Example 1, Comparative Example 2, and Example 1. The interlaminar shear strength of the prepared carbon fiber reinforced polypropylene composites was measured, and the results are as follows: Figure 1 As shown.
[0080] It can be seen that the composite material prepared with the modified carbon fiber in Example 1 exhibits the highest interlaminar shear strength, increasing by 119.35% compared to the untreated composite. This is because the hemispherical PEI nanoparticles form a mechanical interlocking effect with the polypropylene resin. When the composite is subjected to stress failure, crack propagation at the interface is hindered by the PEI nanoparticles. Interface failure requires more energy, and the cracks mainly extend along the resin rather than the interface, thus improving the interlaminar properties of the composite. However, the interlaminar shear strength of the composites prepared with the modified carbon fiber in Comparative Examples 1 and 2 does not show a significant increase compared to the untreated composite. This indicates that the mechanical interlocking effect between the PEI nanoparticles and the resin is strongest only when the PEI nanoparticles are hemispherical, resulting in the best interlaminar properties of the composite.
[0081] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for modifying the surface of carbon fiber, characterized in that, Includes the following steps: The desized carbon fiber was placed in a polyetherimide solution and sonicated at -5 to 3°C for 10 to 30 minutes, and then kept at the temperature for 20 to 30 hours. After the standing period, it was taken out and evaporated at 20°C. The mass concentration of the polyetherimide solution was 0.1 to 0.6 wt%.
2. The carbon fiber surface modification method as described in claim 1, characterized in that, The method for preparing the desized carbon fiber is as follows: heat the carbon fiber to 400~500℃ in an inert gas atmosphere, keep it at that temperature for 1~2 hours, cool it to room temperature, wash it, and dry it to obtain the carbon fiber.
3. The carbon fiber surface modification method as described in claim 2, characterized in that, The inert gas includes one or both of nitrogen and argon; the solvent used in the washing step is water or ethanol.
4. The carbon fiber surface modification method as described in claim 1, characterized in that, Before placing the desized carbon fiber in the polyetherimide solution, the desized carbon fiber is pre-impregnated with the solvent of the polyetherimide solution for 10-30 minutes.
5. The carbon fiber surface modification method as described in claim 1, characterized in that, The ratio of the desized carbon fiber to the polyetherimide solution is 1g:300~700mL.
6. The carbon fiber surface modification method as described in claim 1, characterized in that, The solvent of the polyetherimide solution is selected from one or more of N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), or N,N-dimethylacetamide (DMAc).
7. The carbon fiber surface modification method as described in claim 6, characterized in that, The polyetherimide solution is prepared by placing polyetherimide in a solvent and stirring at 60-80°C for 1-4 hours.
8. A modified carbon fiber, characterized in that, It is prepared by the carbon fiber surface modification method according to any one of claims 1 to 7.
9. A carbon fiber reinforced resin matrix composite material, characterized in that, It includes the modified carbon fiber as described in claim 8.
Citation Information
Patent Citations
A method for surface modification of carbon fiber by nano-silica
CN104499270B
Nanoparticle-containing fiber sizing system for carbon fibers
CN107407042B
Polyetherimide aqueous emulsion type carbon fiber sizing agent as well as preparation method and application thereof
CN103757927A
Polyetheretherketone-base composite, preparing method thereof and application thereof in friction reduction and wear resistance
CN104927298A