Alkaline battery seal ring burst pressure testing device and testing method

By improving the alkaline battery sealing ring burst pressure testing device and method, the battery sealing structure is simulated by using annular ridges and annular resting parts. Combined with a detachable center pin and mold core design, the problems of inaccurate test data and easy mold damage are solved, and higher test accuracy and stability are achieved.

CN118032519BActive Publication Date: 2026-11-20NINGBO GP & SONLUK BATTERY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410113921.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-26
Publication Date
2026-11-20
Estimated Expiration
2044-01-26

AI Technical Summary

Technical Problem

Existing alkaline battery sealing ring burst pressure testing devices produce inaccurate test data, have poor stability, and the molds are easily damaged, making it difficult to meet high-requirement quality control management.

Method used

The system employs a combination structure of lower mold, mold core, center pin, and upper mold. It simulates the battery sealing structure through annular ridges and annular resting parts. Combined with the detachable center pin and mold core design, it ensures the authenticity and stability of the test and improves the assembly accuracy through positioning fixtures.

Benefits of technology

It improves the authenticity, accuracy and stability of test data, reduces the frequency of mold damage, extends the service life of the device, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118032519B_ABST
    Figure CN118032519B_ABST
Patent Text Reader

Abstract

The application discloses a device and a method for testing the burst pressure of a sealing ring of an alkaline battery. The device more realistically simulates the formation of a current collector, the sealing structure of a battery, and the state of the force acting on the sealing ring in the battery by means of an annular ridge and an annular resting portion. The device restores the forming process of the battery by combining the sealing ring with a mold core and then with a lower mold. The mold core with a center pin is combined with the sealing ring with the support of the lower side of the center column of the sealing ring to avoid damage to the explosion-proof structure of the sealing ring. The device further improves the authenticity, accuracy, and stability of the test. The detachable connection of the center pin and the mold core improves the processing convenience, reduces the overall scrap frequency of the mold core, prolongs the service life of the device, reduces the cost, and improves the test stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of quality control of alkaline battery components, and more particularly to an alkaline battery sealing ring burst pressure testing device and testing method. Background Technology

[0002] In alkaline batteries, the sealing ring is a combination of the sealing mechanism and the explosion-proof mechanism of the entire system. With the development of alkaline batteries, the overall structure of the sealing ring has also become more mature, basically presenting the structure shown in patents such as those with authorization announcement numbers CN217740659U, CN217214906U, CN216750103U, CN208835155U, CN205666264U, and CN105958078B.

[0003] like Figure 1 As shown, the sealing ring 500 is a rotating body, which includes a central column 51 for inserting conductor pins 600, an outer peripheral portion 56 that is tightly fitted to the inner wall of the battery casing, and a connecting portion 52 located between the central column 51 and the outer peripheral portion 56; the front of the connecting portion 52 is provided with an annular protrusion 53, the separator paper 800 roll is located inside the annular protrusion 53, and the connecting portion 52 inside the annular protrusion 53 is provided with a thin film-shaped explosion-proof structure 54.

[0004] The negative electrode bottom cover 700, which mates with the sealing ring, is cap-shaped and includes a top wall 71, an annular side wall 72, and a bent brim 73. Vent holes are provided on the top wall 71 or the annular side wall 72. A conductor pin 600 is vertically connected to the top wall 71. The negative electrode bottom cover 700 is embedded from the back of the sealing ring into the annular outer periphery 56 of the sealing ring. The conductor pin 600 is interference-fitted into the central hole of the central column 51 and extends towards the front of the sealing ring.

[0005] During battery encapsulation, the shoulder 55 formed by the outer periphery 56 of the sealing ring and the connecting portion 52 is supported on the annular inner protrusion 91 formed by the groove of the steel shell 900; the rolled edge of the steel shell 900 bends the upper edge of the outer periphery 56 of the sealing ring and presses it onto the brim 73 of the negative electrode bottom cover 700.

[0006] Because the burst pressure of the sealing ring is related to the battery's sealing performance and safety, the range of burst pressure differences is usually limited to within 1 Pa. Furthermore, the burst pressure increases as the battery diameter decreases; for large-volume batteries, the burst pressure value is lower, and higher stability requirements are needed.

[0007] The authorization announcement number CN201892639U discloses a testing device for the sealing ring explosion-proof pressure test device of an alkaline battery. The sealing ring pressure test mold includes a base, a mold core, and a pressure cap. The base is cylindrical with threads on its outer circumference and a cavity in the center for placing the sealing ring. There is an air channel at the bottom of the base, with air inlet and outlet at both ends. The mold core is cylindrical with a pressure block at its bottom. The pressure cap is cylindrical, and its inner wall has threads that mate with the threads on the base.

[0008] The inventors discovered the following problems with the above structure when using the testing device described in the aforementioned patent:

[0009] First, the pattern of the burst pressure of the sealing ring detected by the pressure testing mold of this structure does not correspond to the pattern of the current collector pressure and sealing pressure detected after the actual battery is formed, and the authenticity of the test data is questionable.

[0010] Secondly, the burst pressure test stability of the sealing rings injected into the same cavity within a similar time period is poor and cannot meet the test requirements, so there is no way to use this as a basis for higher quality control management.

[0011] Third, after the burst pressure test is completed, the center pin of the mold core is inserted into the center hole of the sealing ring. Therefore, it is necessary to use tools such as pliers to separate the center pin from the sealing ring. As a result, the center pin is very easy to bend and break, which leads to errors in subsequent tests and even scrapping of the mold. Summary of the Invention

[0012] To address the problems in the prior art, this invention provides an alkaline battery sealing ring burst pressure testing device that is accurate, stable, and has a long service life, and also provides an alkaline battery sealing ring burst pressure testing method that is easy to operate, accurate, and has good repeatability.

[0013] To address the first and second problems of the existing technology, this invention provides a method for testing the burst pressure of an alkaline battery sealing ring; the technical solution adopted to solve the above technical problems is: a method for testing the burst pressure of an alkaline battery sealing ring, including equipment preparation steps and test operation steps;

[0014] The equipment preparation steps include the following:

[0015] Step S1: Connect the lower mold to the test host. The upper end of the lower mold is provided with a groove. The longitudinal air passage below the groove is connected to the air passage of the test host. The groove includes a large diameter section on the upper side and a small diameter section on the lower side. The junction of the large diameter section and the small diameter section forms an annular resting part.

[0016] The test operation steps include the following steps in sequence:

[0017] Step P1: With the central column of the sealing ring supported on the lower side, combine the mold core with the sealing ring and the central pin; the annular ridge at the lower end of the mold core is inserted downward into the outer periphery of the sealing ring with the back side facing upward, and the central pin is inserted into the central hole of the central column and extends towards the front of the sealing ring, thereby simulating the structure of the battery current collector.

[0018] Step P2: Place the mold core with the sealing ring embedded into the mold core cavity of the upper mold with the sealing ring facing downwards; the upper mold has an air vent, which is connected to the longitudinal air vent of the mold core, and the opening of the longitudinal air vent is located inside the annular ridge;

[0019] Step P3: Twist the upper and lower molds to press down the mold core; the sealing ring enters the groove, the outer periphery of the sealing ring is in close contact with the groove wall of the large diameter section, and the shoulder of the sealing ring rests on the annular resting part, thereby simulating the battery sealing structure;

[0020] Step P4: Turn on the air intake switch of the test host, turn the handle of the air pressure regulating valve to gradually increase the air pressure. When the air pressure reaches the burst pressure of the sealing ring, the explosion-proof structure is broken. The test result display shows the burst pressure value.

[0021] To address the third problem existing in the prior art, the preferred technical solution adopted by the present invention to solve the above-mentioned technical problem is as follows: the equipment preparation step further includes the following steps:

[0022] Step S2: Insert the center pin into the longitudinal pin hole of the mold core with its lower end extending out of the end face of the mold core, and fix the center pin to the mold core with a fastening screw through the transverse threaded fixing hole;

[0023] The order of steps S1 and S2 is not important.

[0024] The preferred technical solution adopted by the present invention to solve the above-mentioned technical problems further includes: in step P1, the combination of the sealing ring and the mold core with the center pin is realized by positioning tooling;

[0025] The positioning fixture includes a support base plate, the support base plate includes a support groove, the support groove is provided with an annular support wall and a central support column, and the central support column is provided with a clearance hole in the middle.

[0026] The sealing ring is placed with its reverse side facing up in the support groove of the positioning fixture. The shoulder of the sealing ring is supported by the annular support wall, and the central column of the sealing ring is supported by the central support column. During the process of inserting the mold core, the central pin is cleared through the clearance hole.

[0027] The preferred technical solution adopted by the present invention to solve the above-mentioned technical problems further includes: the upper mold includes a connecting hole located on the front side of the mold core cavity, and the height of the connecting hole is less than the height of the main body of the mold core;

[0028] In step P3, the upper mold is placed on the lower mold, and the mold core is blocked by the upper end face of the lower mold and does not completely detach from the mold core cavity.

[0029] The preferred technical solution adopted by the present invention to solve the above-mentioned technical problems further includes: the lower mold includes a lower base and an upper base, wherein the diameter of the lower base is larger than that of the upper base so that the upper end surface of the lower base forms an annular limiting wall;

[0030] The outer peripheral surface of the upper base includes a lower threaded wall; the lower end of the upper mold includes a connecting hole, and the inner wall of the connecting hole includes an upper threaded wall, an upper smooth wall and a flared guide wall from top to bottom;

[0031] Step P3 includes the following sub-steps:

[0032] Step P31: When the upper mold with the mold core is tilted at a certain angle and the upper mold is obliquely fastened to the lower mold through the flared guide wall, the upper mold is straightened;

[0033] Step P32: Under the action of gravity, the upper smooth wall of the upper mold slides down the upper base of the lower mold until the upper threaded wall and the lower threaded wall come into contact.

[0034] Step P33: Twist the upper mold until the lower end face of the upper mold abuts against the annular limiting wall. Step P3 is then complete.

[0035] The preferred technical solution adopted by the present invention to solve the above-mentioned technical problems further includes: a test termination step.

[0036] The test completion steps include the following:

[0037] Step T1: Acquire burst pressure data and shut off the air intake switch;

[0038] Step T2: Unscrew the upper mold to separate the sealing ring from the mold core and the center pin;

[0039] The lower end of the center pin is provided with a conical tip; in step P1, the rear section of the conical tip is located inside the front section of the central column of the sealing ring;

[0040] In step T2, the sealing ring is pulled off the mold core by using a clamping tool to hold the front part of the central column of the sealing ring.

[0041] In view of the problems one to three in the existing technology, the present invention provides an alkaline battery sealing ring burst pressure testing device; the technical solution adopted to solve the above technical problems is: an alkaline battery sealing ring burst pressure testing device, including a lower mold, a mold core, a center pin and an upper mold;

[0042] The upper mold is a hollow structure with an open lower end. From top to bottom, it includes an air vent, a mold core cavity, and a connecting hole with internal threads. The inner diameter of the mold core cavity is smaller than that of the connecting hole.

[0043] The mold core includes a main body and an annular ridge at the lower end of the main body. The main body is provided with a longitudinal pin hole located in the center and extending vertically, a transverse threaded fixing hole, and a longitudinal air hole. The opening of the longitudinal air hole is located inside the annular ridge. The height of the connecting hole is less than the height of the main body.

[0044] The center pin is inserted into the longitudinal pin hole of the mold core and its lower end extends out of the end face of the mold core. The fastening screw fixes the center pin to the mold core through the threaded fixing hole.

[0045] The lower mold includes an upper base and a lower base connected to the test host. The diameter of the lower base is larger than that of the upper base so that the upper end face of the lower base forms an annular limiting wall. The outer peripheral surface of the upper base is provided with an external thread that matches the connecting hole.

[0046] The upper end of the upper substrate is provided with a groove for accommodating the sealing ring; the groove includes a large-diameter section on the upper side and a small-diameter section on the lower side, and the junction of the large-diameter section and the small-diameter section forms an annular resting part, and the height of the large-diameter section is less than or equal to the height of the outer periphery of the sealing ring.

[0047] The technical solution adopted by the present invention to solve the above-mentioned technical problems further includes: during testing, the sealing ring is located in the groove with its back facing upwards, the outer periphery of the sealing ring is in close contact with the groove wall of the large diameter section, the shoulder of the sealing ring rests on the annular resting part, the annular ridge of the mold core is inserted into the outer periphery of the sealing ring, the connecting part of the sealing ring is clamped by the annular resting part and the annular ridge, the central pin is inserted into the central hole of the central column of the sealing ring and extends towards the front of the sealing ring, and the sealing ring and the lower mold constitute a sealing system.

[0048] The preferred technical solution adopted by the present invention to solve the above-mentioned technical problems further includes: the center pin is a standard needle gauge with a tapered tip at the lower end, and the rear section of the tapered tip is located in the front section of the central column of the sealing ring.

[0049] The preferred technical solution adopted by the present invention to solve the above-mentioned technical problems further includes: the inner wall of the connecting hole includes, from top to bottom, an upper threaded wall, an upper smooth wall and a flared guide wall;

[0050] The outer peripheral surface of the upper substrate includes a constricted guide wall and a lower threaded wall from top to bottom; the threads of the upper threaded wall and the lower threaded wall are mutually matched single-start parallel threads.

[0051] Compared with the prior art, the advantages of the present invention are: by setting the annular ridge and the annular resting part, the formation mode of the current collector and the sealing structure of the battery are simulated more realistically, and the state of the force exerted on the sealing ring inside the battery is restored, thereby providing a strong guarantee for the authenticity, accuracy, stability and repeatability of the test data.

[0052] The battery molding process is replicated by first assembling the sealing ring and the mold core, and then combining them with the lower mold. With the central pillar of the sealing ring supported on its underside, the mold core with the central pin is assembled with the sealing ring, preventing damage to the sealing ring's explosion-proof structure. This further improves the realism, accuracy, and stability of the test.

[0053] The detachable connection between the center pin and the mold core improves processing convenience, reduces the overall scrap frequency of the mold core, extends the service life of the device, reduces costs, and improves testing stability. Attached Figure Description

[0054] The present invention will be further described in detail below with reference to the accompanying drawings and preferred embodiments. However, those skilled in the art will understand that these drawings are drawn only for the purpose of explaining the preferred embodiments and therefore should not be construed as limiting the scope of the invention. Furthermore, unless specifically indicated, the drawings are only schematic representations of the composition or structure of the described objects and may contain exaggerated depictions, and the drawings are not necessarily drawn to scale.

[0055] Figure 1 This is a schematic diagram of the structure of an alkaline battery;

[0056] Figure 2 A schematic diagram of an alkaline battery sealing ring burst pressure testing device;

[0057] Figure 3 An exploded view of an alkaline battery sealing ring burst pressure testing device;

[0058] Figure 4 A schematic diagram of the upper mold of an alkaline battery sealing ring burst pressure testing device;

[0059] Figure 5 A cross-sectional view of the upper mold of an alkaline battery sealing ring burst pressure testing device;

[0060] Figure 6 A schematic diagram of the mold core for a test device to measure the burst pressure of an alkaline battery sealing ring;

[0061] Figure 7Cross-section of the mold core for an alkaline battery sealing ring burst pressure testing device Figure 1 ;

[0062] Figure 8 Cross-section of the mold core for an alkaline battery sealing ring burst pressure testing device Figure 2 ;

[0063] Figure 9 A schematic diagram of the lower mold of an alkaline battery sealing ring burst pressure testing device;

[0064] Figure 10 Diagram showing the operational status of an alkaline battery sealing ring burst pressure testing device;

[0065] Figure 11 This is a diagram showing the usage status of the mold core for the alkaline battery sealing ring burst pressure testing device.

[0066] Figure label:

[0067] Sealing ring 500; Conductor pin 600; Negative electrode bottom cover 700; Separator paper 800; Steel shell 900;

[0068] Central column 51; outer periphery 56; connecting part 52; annular protrusion 53; shoulder 55;

[0069] Top wall 71; circumferential side wall 72; brim 73;

[0070] Annular inner convex body 91;

[0071] Lower mold 100; mold core 200; center pin 300; upper mold 400;

[0072] Vent hole 41; Mold core cavity 42; Connecting hole 43; Main body 21; Annular ridge 22; Longitudinal pin hole 23; Threaded fixing hole 24; Longitudinal air hole 25; Fastening screw D;

[0073] Upper substrate 101; lower substrate 102; annular limiting wall 11; conical tip 31;

[0074] Groove 12; Large diameter section 121; Small diameter section 122; Annular support part 123;

[0075] Inner fillet r1; outer fillet r2; tapered tip 31; annular boss 26;

[0076] Upper threaded wall 431; Upper smooth wall 432; Flared guide wall 433;

[0077] Narrowing guide wall 1011; Lower threaded wall 1012; Countersunk groove W; Clamping plane Z;

[0078] Positioning fixture M; Support base plate M1; Support groove e; Annular support wall f; Central support column y; Clearance hole g; Detailed Implementation

[0079] Preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings. Those skilled in the art will appreciate that these descriptions are merely descriptive and exemplary and should not be construed as limiting the scope of the invention.

[0080] In the description of this invention, it should be noted that the terms "upper," "lower," "front," "rear," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship in which the product of this invention is usually placed when in use. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting this invention.

[0081] This embodiment provides an alkaline battery sealing ring burst pressure testing device, which can be applied to alkaline battery sealing ring burst pressure testing equipment similar to that described in authorization announcement number CN202033255U.

[0082] like Figure 2-3 As shown, specifically, the alkaline battery sealing ring burst pressure testing device includes a lower mold 100, a mold core 200, a center pin 300, and an upper mold 400. The center pin 300 is disposed on the mold core 200, the mold core 200 is assembled inside the upper mold 400, and the upper mold 400 cooperates with the lower mold 100.

[0083] Among them, such as Figure 4-5 As shown, the upper mold 400 is a hollow structure with an open lower end. From top to bottom, it includes an air vent 41, a mold core cavity 42, and a connecting hole 43 with internal threads. The upper end of the air vent 41 extends to the upper surface of the upper mold 400, and the lower end connects to the mold core cavity 42. The air vent 41 can be a single hole located in the center, or it can be an annular channel or a multi-hole structure. The inner diameter of the mold core cavity 42 is smaller than that of the connecting hole 43, and the mold core cavity 42 and the connecting hole 43 have a stepped structure.

[0084] like Figure 3 , 6 As shown in Figure 8, the mold core 200 includes a main body 21 and an annular ridge 22 at the lower end of the main body 21. The inner and outer diameters of the annular ridge 22 are consistent with the dimensions of the negative electrode bottom cover 700 that matches the sealing ring. The outer diameter of the annular ridge 22 is consistent with the outer diameter of the brim 73 of the negative electrode bottom cover 700, and the inner diameter of the annular ridge 22 is consistent with the inner diameter of the annular sidewall 72 of the negative electrode bottom cover 700.

[0085] This design utilizes the mold core 200 to simulate the negative electrode bottom cover 700, restoring the state of the sealing ring under the force of the negative electrode bottom cover 700 inside the battery, thereby providing a strong guarantee for the authenticity and accuracy of the test data.

[0086] As shown in the figure, the height of the connecting hole 43 is less than the height of the main body 21. This arrangement ensures that when the upper mold 400, which contains the mold core 200, is placed on the lower mold 100, the mold core 200 falls due to gravity. When the lower end of the mold core 200 falls onto the upper mold 400, the upper end of the mold core 200 does not detach from the mold core cavity 42, thus keeping the mold core cavity 42 in the correct position at all times.

[0087] like Figure 6-8 As shown, the main body 21 of the mold core 200 has a longitudinal pin hole 23 located in the center and extending vertically, a transverse threaded fixing hole 24, and a longitudinal air hole 25. The lower opening of the longitudinal air hole 25 is located inside the annular ridge 22. The center pin 300 is inserted into the longitudinal pin hole 23 of the mold core 200 and its lower end extends out of the end face of the mold core 200. The fastening screw D fixes the center pin 300 to the mold core 200 through the threaded fixing hole 24.

[0088] When the fastening screw D is removed, the center pin 300 can be pulled out of the mold core 200 to replace it with a new center pin 300. During testing, the center pin 300 is inserted into the central hole of the central post 51 of the sealing ring and extends towards the front of the sealing ring. This arrangement more realistically simulates the structure of the current collector.

[0089] It should be understood that, assuming the center pin 300 and the mold core 200 are a single component, there is a sudden change in diameter between the mold core 200 and the center pin 300. The center pin 300, due to its small diameter and high precision requirements, is difficult to machine. Furthermore, because the center pin 300 is prone to wear and requires special heat treatment, this necessitates processing the entire mold core 200. Under these conditions, the heat treatment effect is not ideal, and the hardness and strength of both the mold core 200 and the center pin 300 will be affected.

[0090] By setting the center pin 300 and the mold core 200 as separate structures, the center pin 300 can be easily machined and heat-treated separately. It can be made of a different material than the body 21 to meet the requirements for its strength and wear resistance. Even high-strength and high-wear-resistant standard needle gauges such as bearing steel needle gauges can be used.

[0091] The center pin 300 and the mold core 200 are detachably connected by the transverse fastening screw D. This not only has a simple structure and is easy to process, but also makes disassembly and installation convenient. The extension length of the center pin 300 can also be adjusted according to needs.

[0092] like Figure 3 , 9As shown, the lower mold 100 includes an upper base 101 and a lower base 102 connected to the test host. The diameter of the lower base 102 is larger than that of the upper base 101 so that the upper end face of the lower base 102 forms an annular limiting wall 11. The outer peripheral surface of the upper base 101 is provided with an external thread that matches the connecting hole 43. The upper end of the upper base 101 is provided with a groove 12 for accommodating a sealing ring. The groove 12 includes a large-diameter section 121 on the upper side and a small-diameter section 122 on the lower side. The junction of the large-diameter section 121 and the small-diameter section 122 forms an annular resting part 123.

[0093] During testing, such as Figure 1 , 10 As shown, the sealing ring is located in the groove 12 with its back facing upwards. The outer periphery 56 of the sealing ring is in close contact with the groove wall of the large diameter section 121. The shoulder 55 of the sealing ring rests on the annular resting part 123. The annular ridge 22 of the mold core 200 is inserted into the outer periphery 56 of the sealing ring. The connecting part 52 of the sealing ring is clamped by the annular resting part 123 and the annular ridge 22. The sealing ring and the lower mold 100 form a sealing system.

[0094] In this structure, the annular resting part 123 simulates the annular inner protrusion 91 formed by the groove of the steel shell 900, and the structure in which the connecting part 52 of the sealing ring is sandwiched by the annular resting part 123 and the annular ridge 22 simulates the sealing structure of the battery, thereby making the test data more consistent with the burst pressure data reflected by the sealing ring in the battery.

[0095] like Figure 1 , 2 As shown in Figure 10, after the upper mold 400 and the lower mold 100 are connected, the annular limiting wall 11 acts as a restriction for screwing into place, so that the test device and the sealing ring are in a relatively uniform state each time, thereby ensuring the stability and repeatability of the test.

[0096] like Figure 9 , 10 As shown, the height of the large-diameter section 121 is less than or equal to the height of the outer periphery 56 of the sealing ring. This causes the upper edge of the outer periphery 56 of the sealing ring to extend beyond the upper end face of the lower mold 100, facilitating its removal from the groove 12.

[0097] like Figure 7 As shown, preferably, the end face of the annular ridge 22 has an inner rounded corner r1 between it and the inner wall of the annular ridge 22, and an outer rounded corner r2 between it and the outer wall of the annular ridge 22. The annular ridge 22 is flared, which can avoid the mold core 200 from squeezing and damaging the sealing ring, and also well simulates the structure of the brim 73 of the negative electrode bottom cover 700.

[0098] like Figure 10As shown, preferably, the center pin 300 has a tapered tip 31 at its lower end, thus forming a structure similar to the conductive nail 600, which facilitates insertion into the central column 51 of the sealing ring.

[0099] More preferably, the rear section of the conical tip 31 is located within the front section of the central pillar 51 of the sealing ring. This is because after the sealing ring bursts, the central pillar 51 may detach from the connecting part 52 of the sealing ring and remain at the lower end of the central pin 300. In this case, the conical tip 31 facilitates the detachment of the central pillar 51 from the central pin 300 along the conical surface of the conical tip 31. It also helps to create a deformation space between the central pillar 51 and the central pin 300 when the front section of the central pillar 51 is clamped with a tool, thus avoiding excessive force acting on the central pin 300 and causing deformation of the central pin 300.

[0100] like Figure 8 As shown, in this embodiment, considering both ease of processing and uniformity of air output, the mold core 200 is provided with two longitudinal air holes 25. The two longitudinal air holes 25 are located on both sides of the longitudinal pin hole 23 and are symmetrically arranged along the central axis. It should be noted that longitudinal air holes 25 with an annular cross-section surrounding the longitudinal pin hole 23 are more preferred.

[0101] Preferably, such as Figure 7 As shown, transverse threaded fixing holes 24 are symmetrically provided on both sides of the mold core 200. Two fastening screws D press against the center pin in the longitudinal pin hole 23, thereby improving the stability of the center pin.

[0102] The outer peripheral wall of the preferred mold core 200 is provided with a countersunk hole to avoid the effect of the limiting head of the fastening screw D on the diameter of the mold core 200.

[0103] like Figure 7-8 As shown in Figure 10, the lower end face of the mold core 200 has an annular boss 26 in the middle surrounding the opening of the longitudinal pin hole 23. This annular boss 26 presses against the end face of the central column 51 on the back of the sealing ring during testing, preventing the sealing ring from bulging upwards as a whole. This is consistent with the function of the head of the conductive nail 600 on the sealing ring in the battery sealing.

[0104] like Figure 3 , 4 As shown in Figure 5, the inner wall of the connecting hole 43 includes, from top to bottom, an upper threaded wall 431, an upper smooth wall 432, and a flared guide wall 433. The outer peripheral surface of the upper base 101 includes, from top to bottom, a constricted guide wall 1011 and a lower threaded wall 1012.

[0105] The flared guide wall 433 and the narrowed guide wall 1011 facilitate the alignment and assembly of the upper mold 400 and the lower mold 100, improving testing convenience.

[0106] Preferably, the threads of the upper threaded wall 431 and the lower threaded wall 1012 are mutually matched single-start parallel threads. The bursting of the sealing ring exerts a strong upward force on the upper mold 400, and the meshing of the single-start parallel threads can prevent the thread pitch from shifting, thereby reducing the possibility of thread damage and improving the service life of the device.

[0107] The upper smooth wall 432 ensures that the upper die 400 and lower die 100 remain coaxial before screwing, avoiding the impact of skewed screwing on the test and damage to the thread structure. Moreover, the upper smooth wall 432 reduces the number of screwing turns while maintaining the sleeve distance, enhancing connection stability and airtightness, thus improving testing convenience and efficiency.

[0108] Preferably, such as Figure 3 As shown, the upper end of the mold core 200 is provided with a groove W, and the upper opening of the longitudinal air hole 25 is located in the groove W. The groove W ensures that no matter what angle the mold core 200 and the upper mold 400 are assembled at, the gas flow of the longitudinal air hole 25 can reach the air outlet 41 of the upper mold 400, thus avoiding air passage blockage.

[0109] like Figure 2 As shown, the upper mold 400 and the lower mold 100 are screwed together to form a cylinder. The lower base 102 has clamping planes Z on both sides, which facilitates the disassembly and installation of the lower mold 100 using a wrench or other tools. More preferably, the outer periphery of the upper mold 400 is provided with anti-slip patterns to facilitate gripping and screwing operations by the operator.

[0110] The method for conducting burst pressure tests on alkaline battery sealing rings using the aforementioned device includes equipment preparation steps and test operation steps.

[0111] The equipment preparation steps include the following:

[0112] Step S1: Connect the lower mold 100 to the test host. The upper end of the lower mold 100 is provided with a groove 12. The longitudinal air passage below the groove 12 is connected to the air passage of the test host. The groove 12 includes a large diameter section 121 on the upper side and a small diameter section 122 on the lower side. The junction of the large diameter section 121 and the small diameter section 122 forms an annular resting part 123.

[0113] Step S2: Insert the center pin 300 into the longitudinal pin hole 23 of the mold core 200 with its lower end extending out of the end face of the mold core 200, and use the fastening screw D to fix the center pin 300 to the mold core 200 through the transverse threaded fixing hole 24.

[0114] The order of steps S1 and S2 is not important.

[0115] Of course, in the following method, the mold core 200 and the center pin 300 are integrated into one unit, so those skilled in the art can also operate with the mold core 200 which has the center pin 300 integrated into one unit.

[0116] The test operation steps include the following steps in sequence:

[0117] Step P1: With the central pillar 51 of the sealing ring supported on its lower side, the mold core 200 with the central pin 300 is assembled with the sealing ring. The annular ridge 22 at the lower end of the mold core 200 is inserted downward into the outer periphery 56 of the sealing ring with its back facing upward. The central pin 300 is inserted into the central hole of the central pillar 51 and extends towards the front of the sealing ring, thereby simulating the structure of the battery current collector.

[0118] Step P2: Place the mold core 200 with the sealing ring embedded into the mold core cavity 42 of the upper mold 400 with the sealing ring facing downwards. The upper mold 400 has an air vent 41, which communicates with the longitudinal air vent 25 of the mold core 200. The opening of the longitudinal air vent 25 is located within the annular ridge 22.

[0119] Step P3: Twist the upper mold 400 and the lower mold 100 to press down the mold core 200. The sealing ring enters the groove 12, and the outer periphery 56 of the sealing ring is in close contact with the groove wall of the large diameter section 121. The shoulder 55 of the sealing ring rests on the annular resting part 123, thereby simulating the battery sealing structure.

[0120] Step P4: Turn on the air intake switch of the test host, turn the handle of the air pressure regulating valve to gradually increase the air pressure. When the air pressure reaches the burst pressure of the sealing ring, the explosion-proof structure 54 is broken. The test result display shows the value of the burst pressure.

[0121] Preferably, in step P1, the method is as follows: Figure 11 The positioning fixture M shown realizes the combination of the sealing ring and the mold core 200 with the center pin 300.

[0122] like Figure 11 As shown, the positioning fixture M includes a support base plate M1, which includes a support groove e. The support groove e contains an annular support wall f and a central support column y. The central support column y has a clearance hole g in its center. The sealing ring is placed with its reverse side facing upwards within the support groove e of the positioning fixture M. The shoulder 55 of the sealing ring is supported by the annular support wall f, and the central column 51 of the sealing ring is supported by the central support column y. During the insertion of the mold core 200, the central pin 300 is cleared through the clearance hole g. This method simulates the current collector assembly process, improving assembly accuracy and avoiding stress damage to the thin-film explosion-proof structure 54 of the sealing ring.

[0123] In step P3, the upper mold 400 is placed on the lower mold 100, and the mold core 200 is blocked by the upper end face of the lower mold 100 and does not completely detach from the mold core cavity 42.

[0124] Step P3 includes the following sub-steps:

[0125] Step P31: When the upper mold 400 with the mold core 200 is tilted at a certain angle, and the upper mold 400 is obliquely fastened to the lower mold 100 through the flared guide wall 433, the upper mold 400 is guided to be straightened.

[0126] Step P32: Under the action of gravity, the upper smooth wall 432 of the upper mold 400 slides down the upper base 101 of the lower mold 100 until the upper threaded wall 431 and the lower threaded wall 1012 come into contact.

[0127] Step P33: Twist the upper mold 400 until the lower end face of the upper mold 400 abuts against the annular limiting wall 11. Step P3 is now complete.

[0128] The test method for the burst pressure of alkaline battery sealing rings also includes a test completion step:

[0129] The test completion steps include the following:

[0130] Step T1: Acquire burst pressure data and shut off the air intake switch.

[0131] Step T2: Unscrew the upper mold 400 to separate the sealing ring from the mold core 200 and the center pin 300.

[0132] Preferably, in step P1, the rear section of the conical tip 31 is located inside the front section of the central column 51 of the sealing ring. In step T2, the sealing ring is pulled off the mold core 200 by using a clamping tool to hold the front section of the central column 51 of the sealing ring.

[0133] The above describes the alkaline battery sealing ring burst pressure testing device provided by the present invention. Specific examples have been used to illustrate the principle and implementation of the invention. The descriptions of the above embodiments are only for the purpose of helping to understand the invention and its core ideas. It should be noted that those skilled in the art can make several improvements and modifications to the invention without departing from its principles, and these improvements and modifications also fall within the protection scope of the claims of the present invention.

Claims

1. A device for testing the burst pressure of an alkaline battery sealing ring, characterized in that... Includes the lower mold, mold core, center pin, and upper mold; The upper mold is a hollow structure with an open lower end. From top to bottom, it includes an air vent, a mold core cavity, and a connecting hole with internal threads. The inner diameter of the mold core cavity is smaller than that of the connecting hole. The mold core includes a main body and an annular ridge at the lower end of the main body. The main body is provided with a longitudinal pin hole located in the center and extending vertically, a transverse threaded fixing hole, and a longitudinal air hole. The opening of the longitudinal air hole is located inside the annular ridge. The height of the connecting hole is less than the height of the main body. The center pin is inserted into the longitudinal pin hole of the mold core and its lower end extends out of the end face of the mold core. The fastening screw fixes the center pin to the mold core through the threaded fixing hole. The lower mold includes an upper base and a lower base connected to the test host. The diameter of the lower base is larger than that of the upper base so that the upper end face of the lower base forms an annular limiting wall. The outer peripheral surface of the upper base is provided with an external thread that matches the connecting hole. The upper end of the upper substrate is provided with a groove for accommodating the sealing ring; the groove includes a large-diameter section on the upper side and a small-diameter section on the lower side, and the junction of the large-diameter section and the small-diameter section forms an annular support portion, and the height of the large-diameter section is less than or equal to the height of the outer periphery of the sealing ring; The inner and outer diameters of the annular ridge are consistent with the size design of the negative electrode bottom cover that matches the sealing ring; the outer diameter of the annular ridge is consistent with the outer diameter of the brim of the negative electrode bottom cover, and the inner diameter of the annular ridge is consistent with the inner diameter of the annular sidewall of the negative electrode bottom cover. During testing, the sealing ring is positioned with its back facing upwards within the groove. The outer periphery of the sealing ring is in close contact with the groove wall of the large-diameter section. The shoulder of the sealing ring rests on the annular support. The annular ridge of the mold core is inserted into the outer periphery of the sealing ring. The connecting part of the sealing ring is clamped by the annular support and the annular ridge. The central pin is inserted into the central hole of the central column of the sealing ring and extends towards the front of the sealing ring. The sealing ring and the lower mold constitute a sealing system.

2. The alkaline battery sealing ring burst pressure testing device according to claim 1, characterized in that... The center pin is a standard pin gauge with a tapered tip at the lower end, and the rear section of the tapered tip is located inside the front section of the central column of the sealing ring.

3. The alkaline battery sealing ring burst pressure testing device according to claim 2, characterized in that... The inner wall of the connecting hole, from top to bottom, includes an upper threaded wall, an upper smooth wall, and a flared guide wall; The outer peripheral surface of the upper substrate includes a constricted guide wall and a lower threaded wall from top to bottom; the threads of the upper threaded wall and the lower threaded wall are matching single-start parallel threads.

4. A method for testing the burst pressure of an alkaline battery sealing ring, characterized in that... The alkaline battery sealing ring burst pressure testing device as described in any one of claims 1-3 includes equipment preparation steps and testing operation steps; The equipment preparation steps include the following: Step S1: Connect the lower mold to the test host. The upper end of the lower mold is provided with a groove, and the longitudinal air channel below the groove is connected to the air channel of the test host. The test operation steps include the following steps in sequence: Step P1: With the central column of the sealing ring supported on the lower side, combine the mold core with the sealing ring and the central pin; the annular ridge at the lower end of the mold core is inserted downward into the outer periphery of the sealing ring with the back side facing upward, and the central pin is inserted into the central hole of the central column and extends towards the front of the sealing ring, thereby simulating the structure of the battery current collector. Step P2: Place the mold core with the sealing ring embedded into the mold core cavity of the upper mold with the sealing ring facing downwards; the upper mold has an air vent, which is connected to the longitudinal air vent of the mold core; Step P3: Twist the upper and lower molds to press down the mold core; the sealing ring enters the groove, the outer periphery of the sealing ring is in close contact with the groove wall of the large diameter section, and the shoulder of the sealing ring rests on the annular resting part, thereby simulating the battery sealing structure; Step P4: Turn on the air intake switch of the test host, turn the handle of the air pressure regulating valve to gradually increase the air pressure. When the air pressure reaches the burst pressure of the sealing ring, the explosion-proof structure is broken. The test result display shows the burst pressure value.

5. The method for testing the burst pressure of an alkaline battery sealing ring according to claim 4, characterized in that: The equipment preparation steps also include the following steps: Step S2: Insert the center pin into the longitudinal pin hole of the mold core with its lower end extending out of the end face of the mold core, and fix the center pin to the mold core with a fastening screw through the transverse threaded fixing hole; The order of steps S1 and S2 is not important.

6. The method for testing the burst pressure of an alkaline battery sealing ring according to claim 4, characterized in that: In step P1, the sealing ring and the mold core with the center pin are combined using a positioning fixture. The positioning fixture includes a support base plate, the support base plate includes a support groove, the support groove is provided with an annular support wall and a central support column, and the central support column is provided with a clearance hole in the middle. The sealing ring is placed with its reverse side facing up in the support groove of the positioning fixture. The shoulder of the sealing ring is supported by the annular support wall, and the central column of the sealing ring is supported by the central support column. During the process of inserting the mold core, the central pin is cleared through the clearance hole.

7. The method for testing the burst pressure of an alkaline battery sealing ring according to claim 6, characterized in that: The upper mold includes a connecting hole located on the front side of the mold core cavity; In step P3, the upper mold is placed on the lower mold, and the mold core is blocked by the upper end face of the lower mold and does not completely detach from the mold core cavity.

8. The method for testing the burst pressure of an alkaline battery sealing ring according to claim 6, characterized in that: The outer peripheral surface of the upper base includes a lower threaded wall; the lower end of the upper mold includes a connecting hole, and the inner wall of the connecting hole includes an upper threaded wall, an upper smooth wall and a flared guide wall from top to bottom; Step P3 includes the following sub-steps: Step P31: When the upper mold with the mold core is tilted at a certain angle and the upper mold is obliquely fastened to the lower mold through the flared guide wall, the upper mold is straightened; Step P32: Under the action of gravity, the upper smooth wall of the upper mold slides down the upper base of the lower mold until the upper threaded wall and the lower threaded wall come into contact. Step P33: Twist the upper mold until the lower end face of the upper mold abuts against the annular limiting wall. Step P3 is then complete.

9. The method for testing the burst pressure of an alkaline battery sealing ring according to claim 4, characterized in that: It also includes the test completion steps: The test completion steps include the following: Step T1: Acquire burst pressure data and shut off the air intake switch; Step T2: Unscrew the upper mold to separate the sealing ring from the mold core and the center pin; The lower end of the center pin is provided with a conical tip; in step P1, the rear section of the conical tip is located inside the front section of the central column of the sealing ring; In step T2, the sealing ring is pulled off the mold core by using a clamping tool to hold the front part of the central column of the sealing ring.

Citation Information

Patent Citations

  • battery collector

    CN105958078B

  • Bursting pressure testing device of alkaline battery sealing ring

    CN202033255U

  • Alkaline battery sealing ring

    CN205666264U

  • Improved alkaline battery sealing ring

    CN208835155U

  • Alkaline battery sealing ring and sealing structure

    CN216750103U