Synthesis gas to alcohol catalyst, preparation method and application thereof, and method for synthesizing ethanol and higher alcohol from synthesis gas
By using a composite oxide support to support molybdenum and tungsten sulfides in the syngas-to-alcohol catalyst, combined with surfactants and hydrothermal deposition technology, the problems of insufficient catalyst activity and poor dispersibility were solved, and efficient synthesis of higher alcohols was achieved.
Patent Information
- Application Number
- CN202211379558.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-11-04
AI Technical Summary
Existing catalysts for syngas-to-methanol production suffer from insufficient activity, poor dispersion of metal components, and low syngas conversion rates, making it difficult to achieve high selectivity and high conversion rates for higher alcohols.
Molybdenum and tungsten sulfide catalysts supported on composite oxide supports are used. Through surfactant-assisted hydrothermal deposition and calcination technology, the dispersion and interaction of active components are controlled, and transition metal and alkali metal components are loaded to form a highly dispersed sulfide structure.
This improved the catalyst activity and selectivity for higher alcohols, enhanced the conversion rate of syngas and the selectivity for lower alcohols, and achieved efficient catalyst conversion.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalysts for syngas-to-ethanol production, specifically to a catalyst for syngas-to-ethanol production, its preparation method and application, and a method for producing ethanol and higher alcohols from syngas. Background Technology
[0002] In recent years, due to environmental reasons, methyl tert-butyl ether (MTBE) has been banned as an oil additive in some countries and regions. This has greatly increased the practical value of ethanol and higher alcohols (mainly C2-C4 alcohols) as oil additives. They also have high economic value as liquid fuels, chemicals, and chemical raw materials. If C2-C4 higher alcohols can be produced from syngas derived from coal, natural gas, etc., it can save food, reduce environmental pollution, and to some extent replace the existing petrochemical route based on ethylene hydration, which is of significant research importance.
[0003] Numerous reports exist on the synthesis of low-carbon mixed alcohols from syngas, primarily including modified methanol synthesis catalysts, Cu-Co catalysts, Rh-based catalysts, and molybdenum sulfide-based catalysts. Among these, the molybdenum sulfide-based catalyst was first developed by Dow Chemical Company in the United States (US4882360, EP01192609A). This catalyst consists of molybdenum sulfide, alkali metal / alkaline earth metal, Group VIII metal, and a support, with (NH4)6Mo7O as the catalyst. 24 Using NH3·H2O and NH4S as raw materials, MoS2 is obtained after reaction at a certain temperature. After grinding with bentonite and K2CO3 in a certain proportion, an aqueous solution of cobalt acetate is added, and the mixture is dried and calcined to obtain a composite catalyst. This catalyst has unique anti-sulfur properties, avoiding the requirement for deep desulfurization of the raw gas. At the same time, due to the low water content in the reaction products and the high selectivity for higher alcohols, it is considered one of the most promising catalyst systems for industrial application.
[0004] CN102351641A discloses a method for synthesizing molybdenum-based sulfide catalysts using SBA-15 as a support. The method involves sequentially adding and mixing template agent P123, tetraethyl orthosilicate, (NH4)2MoS4, and cobalt salt, followed by a hydrothermal method to obtain a catalyst precursor. This precursor is then mixed with inorganic potassium salt powder to obtain a catalyst for the synthesis of higher alcohols from syngas. CN1631527A, CN1663683A, and CN1431049A disclose in-depth research conducted by the Shanxi Coal Chemistry Institute of the Chinese Academy of Sciences on molybdenum-based sulfide catalyst systems. CN1631527A discloses a method for obtaining ammonium thiomolybdate through a sulfidation reaction of ammonium sulfide and ammonium molybdate in a concentrated acetic acid system. The ethanol solution of ammonium thiomolybdate is then mixed with an ethanol solution of a transition metal, aged, and washed to obtain a precipitate. After drying, the precipitate is mixed with potassium salt to obtain a molybdenum-based sulfide catalyst. By introducing Mn (CN1663683A) into the above system and adding a binder (bentonite or graphite) for mixing and molding, the stability of the catalyst was improved. CN101428229A discloses a preparation method similar to CN1631527A, which introduces rare earth elements into the catalyst to improve C. 2+ Alcohol selectivity. CN103313785A discloses a method of supporting molybdenum, sulfur, and alkali metal ions on mesoporous carbon molecular sieves via impregnation to improve the selectivity for higher alcohols and ethanol. CN102125857A discloses a method of mixing cobalt nitrate, nickel nitrate, and ammonium molybdate aqueous solutions with carbon nanotubes, adding ammonia to form a precipitate, followed by filtration, washing, drying, and calcination, and then impregnating an equal volume of K2CO3 aqueous solution. After drying and calcination, a cobalt-nickel-molybdenum-potassium catalyst is obtained, achieving a total alcohol-ether carbon-based selectivity of 78%.
[0005] Although alkali metal-modified MoS2-based catalysts are considered one of the most promising advanced alcohol catalyst systems, the conversion rate of syngas in existing technologies remains limited. Further improving the catalytic activity and selectivity of advanced alcohols is key to the industrialization of the synthesis of low-carbon mixed alcohols. Summary of the Invention
[0006] The purpose of this invention is to overcome the problems of insufficient activity of syngas-to-ethanol catalysts, poor dispersion of metal components, and low conversion rate of syngas in the prior art. It provides a syngas-to-ethanol catalyst, its preparation method and application, and a method for producing ethanol and higher alcohols from syngas. The catalyst has a high degree of dispersion of molybdenum and tungsten sulfides, which can improve the utilization rate of metal components and increase the conversion rate of syngas.
[0007] To achieve the above objectives, the present invention provides a syngas-to-methanol catalyst, the catalyst comprising a composite oxide support and a first metal component, a second metal component, and a third metal component supported on the composite oxide support; the first metal component comprises molybdenum and tungsten, wherein, elementally, the molar ratio of molybdenum to tungsten is 1-9:1; the second metal component is selected from at least one transition metal and is different from the first metal component; the third metal component is selected from at least one alkali metal. In the catalyst, the first metal component exists at least partially in the form of sulfides, and the average sheet length of the sulfides of the first metal component is 0.5-10 nm, and the average number of sheet layers is 2-4.
[0008] A second aspect of the present invention provides a method for preparing a catalyst for syngas-to-methanol production, the method comprising: (1) Provide a solution A containing a molybdenum source and a solution B containing a tungsten source; the molar ratio of the molybdenum source to the tungsten source is 1-9:1, based on elemental composition. The pH values of solutions A and B are each independently selected from 1 to 6; (2) Under stirring conditions, a surfactant and solution B are introduced into solution A to obtain a mixture; The surfactant includes a first surfactant and a second surfactant; the first surfactant is selected from C6-C10 alkyl quaternary ammonium salts, and the second surfactant is selected from C12-C20 alkyl quaternary ammonium salts. (3) The above mixture is mixed with the composite oxide carrier, hydrothermal deposition is performed, and then a first calcination is performed to obtain the first precursor; (4) The second metal component and the third metal component are loaded onto the first precursor; the second metal component is selected from at least one transition metal other than molybdenum and tungsten; the third metal component is selected from at least one alkali metal. (5) The product obtained in step (4) is activated by sulfurization.
[0009] A third aspect of the present invention provides a syngas-to-ethanol catalyst prepared by the above-described preparation method.
[0010] The fourth aspect of this invention provides the application of the syngas-to-methanol catalyst described in the first or third aspect in the syngas-to-methanol reaction.
[0011] The fifth aspect of the present invention provides a method for producing ethanol and higher alcohols from syngas, the method comprising: contacting syngas with a catalyst under syngas-to-alcohol reaction conditions; The catalyst is the syngas-to-methanol catalyst described in the first or third aspect.
[0012] The syngas-to-ethanol catalyst provided by this invention features high loading and dispersion of active components and unobstructed support pores. It enables control over the size of the active precursor wafers, weakens the interaction between the active components and the support, increases the synergistic effect of the components, and improves the catalyst's selectivity for higher alcohols. When used in the reaction of syngas to ethanol and higher alcohols, it can improve the conversion rate of syngas and the selectivity for lower alcohols. Detailed Implementation
[0013] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0014] The first aspect of the present invention provides a catalyst for syngas-to-methanol production, the catalyst comprising a composite oxide support and a first metal component, a second metal component, and a third metal component supported on the composite oxide support; the first metal component comprises molybdenum and tungsten, wherein, elementally, the molar ratio of molybdenum to tungsten is 1-9:1; the second metal component is selected from at least one transition metal and is different from the first metal component; the third metal component is selected from at least one alkali metal. In the catalyst, the first metal component exists at least partially in the form of sulfides, and the average sheet length of the sulfides of the first metal component is 0.5-10 nm, and the average number of sheet layers is 2-4.
[0015] According to the present invention, the catalyst has the characteristics of high dispersion of the first metal component and unobstructed support pores, and the interaction between the first metal component and the support is weak, which helps to exert the synergistic effect between the components. The catalyst has high selectivity for higher alcohols.
[0016] The MoS2-based catalyst has a layered crystal structure, with multiple layers of molybdenum sulfide composed of several single layers. Its dispersion is generally characterized in the art by the average length of the metal sulfide lamellars; a smaller average lamellar length indicates higher dispersion of the metal sulfide, while the average number of lamellar layers needs to match the average lamellar length. In existing MoS2-based catalysts, the average lamellar length of the sulfides is large, and the average number of layers is mismatched, resulting in low dispersion and limiting further improvement in catalyst performance. According to the catalyst of the present invention, preferably, the average lamellar length of the sulfide in the first metal component is 4-10 nm, and the average number of lamellar layers is 2-3.
[0017] In this invention, the dispersion of the first metal component is obtained through statistical testing of transmission electron microscopy results. According to the present invention, preferably, the specific surface area of the catalyst is 100-200 m². 2 / g, preferably 120-200m 2 / g, more preferably 160-200 m 2 / g.
[0018] In this invention, the selection range for the content of each component in the catalyst is relatively wide, allowing for a high loading of the first metal component. In the prior art, conventional catalysts exhibit poor metal component dispersion when the loading is high. The inventors of this invention discovered that the interaction between the composite surfactant and the molybdate / tungstenate precursor forms organic-inorganic mixed nanocrystals, promoting high dispersion of the first metal. Preferably, based on the weight of the composite oxide support, the content of the first metal component in the catalyst is 2-50 wt%, preferably 6-20 wt%; the content of the second metal component is 2-20 wt%, preferably 2-10 wt%; and the content of the third metal component is 1-12 wt%, preferably 2-10 wt%. For example, based on elements, the preferred content of the first metal component is any one of 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 12wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, and 20wt%, or a range consisting of any two of the above values. The preferred content of the second metal component is any one of 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, and 10wt%, or a range consisting of any two of the above values. The preferred content of the third metal component is any one of 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, and 10wt%, or a range consisting of any two of the above values.
[0019] According to the present invention, preferably, the molar ratio of the second metal component to the first metal component, based on elemental composition, is 0.2-2.5:1, more preferably 0.5-1.5:1. In the above-mentioned preferred embodiment, it is beneficial to promote the interaction between the second metal and the first metal, thereby increasing the CO conversion rate. However, an excessively high content of the second metal component may lead to an increase in byproducts.
[0020] Preferably, the molar ratio of the third metal component to the first metal component is 0.1-4:1, more preferably 0.5-4:1, based on elemental composition. In the above-mentioned preferred embodiment, this promotes the formation of lower alcohols; however, an excessive amount of the third metal component may lead to a decrease in catalyst activity.
[0021] In this invention, the content of each component is obtained by inductively coupled plasma atomic reflection spectroscopy (ICP-AES).
[0022] According to the present invention, preferably, the molar ratio of molybdenum to tungsten in the catalyst is 1-6:1 (elementally). The inventors of the present invention have discovered that the introduction of tungsten can regulate the interaction between the components in the catalyst, and within the above-mentioned preferred ratio range, can further improve the selectivity of the catalyst for higher alcohols, especially ethanol.
[0023] In this invention, the first metal component exists at least partially in the form of a sulfide. It is understood that the sulfide includes any one or more of molybdenum sulfide, tungsten sulfide, and Mo-WS composite sulfides. The invention does not particularly limit the content of the aforementioned sulfide components; the presence of a portion of the first metal component as a sulfide can improve the catalyst activity. The first, second, and third metal elements in the catalyst can exist in reduced, sulfide, or carbide states. It is understood that in the syngas-to-methanol reaction, the metal elements in the catalyst may react with CO, potentially forming carbides in some cases.
[0024] Preferably, the second metal component is present at least partially in the form of a metal sulfide.
[0025] Preferably, the third metal component is present at least partially in the form of an oxide.
[0026] According to the present invention, preferably, the second metal component is selected from at least one of Group VIII metals, more preferably from at least one of Ni, Co, Mn and Rh; more preferably Ni.
[0027] Preferably, the third metal component is Na and / or K.
[0028] According to a preferred embodiment of the present invention, the first metal component comprises molybdenum and tungsten, the second metal component is Ni, and the third metal component is K. With the above-mentioned preferred catalyst composition, it is advantageous to further improve the catalytic activity of the catalyst and enhance the selectivity of higher alcohols.
[0029] In this invention, the use of a composite oxide support helps improve the dispersibility of the sulfide in the first metal component, weakens the interaction between the active component and the support, increases the synergistic effect of each component, and improves the catalytic activity of the catalyst. Furthermore, the composite oxide simultaneously provides different active sites, which is beneficial for improving the selectivity of the target product. In this invention, the selection range for the composite oxide support is relatively wide; for example, conventional two-component or three-component composite oxide supports in the art can be used. Preferably, the two-component composite oxide support is selected from at least one of MgO-Al2O3, CaO-Al2O3, TiO2-CaO, Al2O3-ZrO2, TiO2-MgO, TiO2-Al2O3, MgO-SiO2, Al2O3-SiO2, and MgO-ZrO2. This invention allows for a wide selection range of the content of the two components in the two-component composite oxide support; the molar ratio of the two components, based on elemental composition, can be 1:0.1-10, preferably 1:0.2-5. Preferably, the three-component composite oxide support is TiO2-MgO-Al2O3 and / or ZrO2-MgO-Al2O3. The present invention does not impose any particular limitation on the content of each component in the three-component composite oxide support. Preferably, the molar ratio of each component, based on elemental composition, can be 1:0.1-10:0.1-10, more preferably 1:0.1-7:0.1-7. Under the above-mentioned preferred composition, it is beneficial to improve the synergistic effect between the composite oxide support and the supported components, which helps to improve the catalytic activity of the catalyst.
[0030] According to the present invention, in order to further improve the dispersion of the sulfide of the first metal component, preferably, the composite oxide support is prepared by co-precipitation in a microchannel.
[0031] A second aspect of the present invention provides a method for preparing a catalyst for syngas-to-methanol production, the method comprising: (1) Provide solution A containing a molybdenum source and solution B containing a tungsten source; the molar ratio of molybdenum source to tungsten source is 1-9:1 (elementally). The pH values of solutions A and B are each independently selected from 1 to 6; (2) Under stirring conditions, a surfactant and solution B are introduced into solution A to obtain a mixture; The surfactant includes a first surfactant and a second surfactant; the first surfactant is selected from C6-C10 alkyl quaternary ammonium salts, and the second surfactant is selected from C12-C20 alkyl quaternary ammonium salts. (3) The above mixture is mixed with the composite oxide carrier, hydrothermal deposition is performed, and then a first calcination is performed to obtain the first precursor; (4) The second metal component and the third metal component are loaded onto the first precursor; the second metal component is selected from at least one transition metal other than molybdenum and tungsten; the third metal component is selected from at least one alkali metal. (5) The product obtained in step (4) is activated by sulfurization.
[0032] In this invention, preferably, in step (1), the pH of solution A and solution B are each independently selected from 2-4.
[0033] Preferably, the pH of solutions A and B is adjusted by introducing an inorganic acid. The present invention does not particularly limit the specific type of the inorganic acid, as long as it can achieve the above-mentioned pH range adjustment; for example, the inorganic acid can be hydrochloric acid and / or nitric acid.
[0034] The present invention allows for a wide range of choices regarding the specific types of molybdenum and tungsten sources, as long as molybdenum and tungsten elements are available. These sources can be any conventional molybdenum-containing soluble salt or tungsten-containing soluble salt, such as soluble molybdates or tungstates. Preferably, the molybdenum source is sodium molybdate and / or ammonium molybdate; preferably, the tungsten source is sodium tungstate and / or ammonium tungstate.
[0035] According to the present invention, solutions A and B each independently include a solvent. The present invention does not particularly limit the specific type of solvent; conventional solvents in the art can be used, for example, water. The present invention also does not impose any particular requirement on the amount of solvent used, as long as it is sufficient to fully dissolve the desired substance. Those skilled in the art can select the appropriate amount based on actual needs.
[0036] Preferably, the molar ratio of molybdenum source to tungsten source is 1-6:1, based on elemental composition.
[0037] According to the present invention, preferably, in step (2), the molar ratio of the amount of surfactant to the total amount of tungsten source and molybdenum source in terms of elements is 0.2-10:1, preferably 1-2:1.
[0038] The inventors of this invention discovered in their research that by combining alkyl quaternary ammonium salt surfactants with different carbon number ranges, the dispersion of the sulfide of the first metal component can be synergistically optimized. Preferably, the molar ratio of the second surfactant to the first surfactant is 0.2-10:1, more preferably 1-5:1.
[0039] In this invention, the first surfactant is selected from C6-C10 alkyl quaternary ammonium salts, and the second surfactant is selected from C12-C20 alkyl quaternary ammonium salts; it is understood that in this invention, the number of carbons refers to the total number of carbons in the compound.
[0040] According to a particularly preferred embodiment of the present invention, the first surfactant is tetraethylammonium bromide and the second surfactant is hexadecyltrimethylammonium bromide. Using this specific combination of surfactants can synergistically improve the dispersion of the sulfide in the first metal component and enhance the catalytic activity of the catalyst.
[0041] According to the present invention, preferably, in step (3), the amount of the mixture and the composite oxide is such that, based on the weight of the composite oxide carrier, the total amount of the molybdenum source and the tungsten source is 2-50 wt%, preferably 6-20 wt%, in terms of molybdenum and tungsten elements.
[0042] In this invention, the selection range for the specific conditions of the hydrothermal deposition is relatively wide. Preferably, the conditions for the hydrothermal deposition include: a reaction temperature of 80-160℃, more preferably 80-120℃, and a reaction time of 5-36 h, more preferably 16-30 h. Under these preferred conditions, the activity of the obtained catalyst can be further improved. In this invention, the hydrothermal deposition is carried out under stirring conditions. This invention does not have special requirements for the specific stirring conditions, and conventional operating conditions in the art can be used.
[0043] According to the present invention, the preparation method further includes: performing solid-liquid separation, washing, and drying on the product obtained by hydrothermal deposition, followed by the first calcination. The present invention does not particularly limit the specific operation methods and conditions for the solid-liquid separation, washing, and drying; those skilled in the art can select them according to actual needs. Preferably, the drying conditions include drying at 80-120°C for 12-24 hours.
[0044] In this invention, preferably, the conditions for the first calcination include: a calcination temperature of 400-600℃, more preferably 450-550℃, and a calcination time of 12-48h, more preferably 24-36h.
[0045] In this invention, there are no particular limitations on the loading method of the second metal component and the third metal component. Conventional methods such as impregnation or dry mixing can be used. The second metal component and the third metal component can be loaded together, or the second metal component can be loaded first and then the third metal component can be loaded. As long as the second metal component and the third metal component can be loaded on the first precursor, those skilled in the art can choose according to actual needs.
[0046] According to a preferred embodiment of the present invention, step (4) includes: (4-1) The second metal component is loaded onto the first precursor by an impregnation method; (4-2) The product obtained in step (4-1) is mixed with the salt of the third metal component to obtain the second precursor.
[0047] The preferred loading method described above is beneficial for promoting the interaction between the various metal components and increasing the yield of the target product.
[0048] According to the present invention, preferably, based on the weight of the composite oxide carrier, the amount of the second metal component is 2-20 wt%, preferably 2-10 wt%, in terms of elements; and the amount of the third metal component is 1-12 wt%, preferably 2-10 wt%.
[0049] Preferably, the molar ratio of the second metal component to the total amount of molybdenum source and tungsten source is 0.2-2.5:1, more preferably 0.5-1.5:1.
[0050] Preferably, the molar ratio of the third metal component to the total amount of molybdenum source and tungsten source is 0.1-4:1, more preferably 0.5-3:1, based on elemental composition.
[0051] According to the present invention, preferably, the second metal component is selected from at least one of Group VIII metals, more preferably from at least one of Ni, Co, Mn and Rh; more preferably Ni.
[0052] Preferably, the third metal component is Na and / or K.
[0053] According to a preferred embodiment of the present invention, the first metal component comprises molybdenum and tungsten, the second metal component is Ni, and the third metal component is K. With the above-mentioned preferred catalyst composition, it is advantageous to further improve the catalytic activity of the catalyst and enhance the selectivity of higher alcohols.
[0054] In this invention, molybdenum and tungsten are at least partially present in sulfide form through the sulfidation activation described in step (5). This invention does not impose any particular limitation on the specific method of sulfidation activation; any conventional sulfidation method in the art can be used. Preferably, in step (5), the sulfidation activation includes contacting the product obtained in step (4) with sulfidation gas. This invention does not impose any particular limitation on the specific conditions of the sulfidation activation; conventional methods and conditions in the art can be used, as long as they are conducive to improving the performance of the catalyst. Preferably, the conditions for sulfidation activation include: a temperature of 300-600℃, preferably 350-450℃; a time of 2-10h, preferably 2-4h; and a volume hourly space velocity of 200-4000h⁻¹. -1 .
[0055] Preferably, the sulfiding gas is a mixture of H2S, H2, and optionally an inert gas. Preferably, the H2S content in the sulfiding gas is 10-20% by volume, and the H2 content is 80-90% by volume. By adopting the above preferred embodiments, the sulfidation activation effect can be further improved, and the activity and selectivity of the catalyst can be enhanced.
[0056] According to the present invention, the selection range of the composite oxide support is the same as that of the composite oxide support in the above-mentioned catalyst, and will not be repeated here.
[0057] According to the present invention, in order to further improve the dispersibility of metal sulfides, preferably, the composite oxide support is prepared by co-precipitation in microchannels.
[0058] Preferably, the method for preparing the composite oxide support includes: S1. A solution containing soluble compounds and a precipitant solution of the composite components are fed into a microchannel reactor in parallel to carry out a precipitation reaction within the microchannel. S2. The product obtained from the above precipitation reaction is aged, dried and calcined.
[0059] In this invention, there are no particular limitations on the solvent in the solution of the soluble compound containing the complex components, as long as it can fully dissolve the soluble compound containing the complex components. For example, the solvent can be water. This invention also does not limit the amount of solvent used, as long as it can dissolve the desired substance. Those skilled in the art can freely choose the amount according to actual needs.
[0060] The present invention allows for a wide range of specific types of soluble compounds containing the composite components, and can employ any conventional combination of soluble salts in the art that satisfies the composition of the aforementioned composite components. For example, when the composite oxide support is MgO-Al2O3, the soluble compound containing the composite components can be a combination of a soluble salt of magnesium and a soluble salt of aluminum.
[0061] The present invention allows for a wide range of choices for the precipitant, as long as the precipitation reaction can occur. Those skilled in the art can select the appropriate precipitant based on actual needs. Preferably, the precipitant is selected from at least one of sodium carbonate, ammonia, sodium bicarbonate, sodium hydroxide, potassium hydroxide, and potassium carbonate, and more preferably sodium hydroxide and / or sodium carbonate. There is no particular limitation on the ratio of sodium hydroxide to sodium carbonate; those skilled in the art can select the appropriate ratio based on actual needs. In this invention, the precipitant is preferably introduced in the form of a solution, and the concentration of the precipitant in the solution is preferably 0.3-2 mol / L. More preferably, it is introduced in the form of an aqueous solution of sodium hydroxide and sodium carbonate.
[0062] The present invention allows for a wide range of selectable conditions for the precipitation reaction. Preferably, the conditions for the precipitation reaction in step S1 include: a precipitation temperature of 10-80℃, more preferably 20-65℃, and a pH value of 6-10, more preferably 7-9. Under these preferred conditions, the activity of the obtained catalyst can be further improved. In the present invention, the precipitation reaction is preferably carried out in a microchannel. The present invention does not limit the method of controlling the precipitation temperature, but it is preferably controlled by a constant temperature water bath.
[0063] In this invention, the liquid flow velocity within the pores of the microchannel reactor can be selected over a wide range. Preferably, the linear velocity of the liquid flow within the pores of the microchannel reactor is not less than 0.05 m / s, more preferably not less than 0.1 m / s, and even more preferably 0.5-100 m / s. For example, it can be 0.5 m / s, 1 m / s, 2 m / s, 3 m / s, 5 m / s, 8 m / s, 9 m / s, 10 m / s, 20 m / s, 60 m / s, 80 m / s, and any range between two values, with 0.5-10 m / s being the most preferred. The inventors of this invention discovered through research that regardless of the liquid flow rate within the channels, as long as the liquid flow linear velocity is within the aforementioned range, it is beneficial to further improve the dispersibility of the catalyst. Further research revealed that when the liquid flow velocity within the channels of the microchannel reactor is ≤100 m / s, fluid control is more efficient; and when the liquid flow velocity within the channels of the microchannel reactor is ≥0.5 m / s, it is more conducive to breaking up the synthesized precipitated particles, thus improving production efficiency. In the preferred embodiment of this invention, the resulting catalyst exhibits higher dispersibility, thereby enhancing catalyst activity.
[0064] The present invention does not impose any particular limitation on the pores of the microchannel reactor, as long as they can meet the aforementioned liquid flow linear velocity. Preferably, the pores of the microchannel reactor are at least one of circular holes, elliptical holes, square holes, and rectangles, and more preferably rectangular.
[0065] Preferably, the channels of the microchannel reactor are rectangular, and the channel dimensions satisfy the following: cross-section of (2mm-10mm) × (0.1mm-2mm), and length of 400mm-1000mm. More preferably, the channel dimensions satisfy the following: cross-section of (3mm-8mm) × (0.2mm-1mm), and length of 500mm-800mm. In this invention, the cross-section refers to the cross-sectional area of the channel, and the cross-sectional dimensions refer to the width and thickness of the cross-section; the length refers to the length of the channel along the direction of liquid flow within the channel. This invention does not limit the number of channels in the microchannel reactor; it can be single-channel or multi-channel, and those skilled in the art can freely choose according to their needs.
[0066] According to the present invention, the aging time in step S2 is 2-24 hours, preferably 2-8 hours; preferably, the aging is carried out under stirring conditions.
[0067] In this invention, the specific conditions for drying and calcination are not particularly limited and can be carried out using conventional methods in the art. Preferably, the drying temperature is 100-250℃ and the drying time is 1-8 hours; more preferably, the drying temperature is 120-180℃ and the drying time is 2-6 hours.
[0068] Preferably, the roasting temperature is 250-850℃, more preferably 350-650℃, and even more preferably 400-500℃; the roasting time is 1-24h, more preferably 2-12h, and even more preferably 3-6h.
[0069] In this invention, step S2 further includes washing the aged product. This invention places no restrictions on the washing method or detergent, as long as it facilitates impurity removal; water is preferred as the detergent.
[0070] A third aspect of the present invention provides a syngas-to-ethanol catalyst prepared by the above-described preparation method.
[0071] The fourth aspect of this invention provides the application of the syngas-to-methanol catalyst described in the first or third aspect in the syngas-to-methanol reaction.
[0072] The fifth aspect of the present invention provides a method for producing ethanol and higher alcohols from syngas, the method comprising: contacting syngas with a catalyst under syngas-to-alcohol reaction conditions; The catalyst is the syngas-to-methanol catalyst described in the first or third aspect.
[0073] According to the present invention, preferably, the reaction conditions for syngas to alcohol production include: a reaction temperature of 250-400℃, a reaction pressure of 2-8MPa, and a syngas volume hourly space velocity of 1000-5000 mL / g / h; preferably, the reaction temperature is 300-350℃, the reaction pressure is 5-7MPa, and the syngas volume hourly space velocity is 2000-3000 mL / g / h.
[0074] Preferably, the volume ratio of CO to H2 in the synthesis gas is 0.5-1:1.
[0075] Preferably, the reaction is carried out under an internal standard of an inert gas, preferably nitrogen.
[0076] Preferably, the volume ratio of the inert gas to the synthesis gas is 0.05-0.1:1.
[0077] The present invention will be described in detail below through embodiments.
[0078] In the following examples and comparative examples, the content of each component was obtained by inductively coupled plasma atomic reflectance spectrometry (ICP-AES).
[0079] Example 1 (1) Prepare a mixed alkaline solution with a NaOH concentration of 1.20 M according to the molar ratio of n(NaOH):n(Na2CO3)=8, and prepare a nitrate (Mg(NO3)2·6H2O, Al(NO3)3·9H2O) solution with a total metal ion concentration of 0.60 M according to the molar ratio of n(Mg):n(Al)=7:3. Add the mixed alkaline solution to the nitrate solution, adjust the pH to 8, and flow into a microchannel reactor under the conditions of 65℃ and thorough stirring. The liquid flow linear velocity in the pores of the microchannel reactor is 2m / s. The pores of the microchannel reactor are rectangular, and the pore dimensions of the microchannel reactor are: cross-sectional dimensions of 3mm×0.5mm and length of 800mm. After the metal salt solution and the alkaline solution are mixed in the microchannel, a uniform suspension is formed. After precipitation, continue stirring and aging for 4 hours. After cooling to room temperature, filter and wash with deionized water until neutral. The filter cake was dried at 120℃ for 6 hours, then calcined at 500℃ for 4 hours, and ground into powder to obtain the MgO-Al2O3 composite oxide carrier.
[0080] (2) Prepare 6.47 mL of 0.22 M Na₂MoO₄ solution A and 2.16 mL of 0.22 M Na₂WO₄ solution B. While stirring, add 2.0 M HCl solution dropwise to adjust the pH of solutions A and B to 5. Then, add 12.6 mL of a pre-prepared 0.15 M tetraethylammonium bromide (TEAB) and hexadecyltrimethylammonium bromide (CTAB) with a molar ratio of 1:3 to solution A dropwise. Subsequently, add solution B to the above solution (molar ratio (CTAB+TEAB):(MoO₄) 2- +WO4 2- MoO4 = 1:1 2- :WO4 2- = 3:1), stirred for 2 hours to obtain a white emulsion suspension, then 1 g of the above MgO-Al2O3 composite oxide carrier was added, transferred to an autoclave, and subjected to hydrothermal deposition reaction at 120℃ for 24 hours. After cooling, the suspension was filtered, washed with water, dried at 120℃ for 10 hours, and calcined at 500℃ for 4 hours to obtain (MoO3+WO3) / MgAl composite oxide.
[0081] (3) Prepare an aqueous solution of nickel nitrate containing 0.14 g (approximately 0.75 mL), and load it by stepwise impregnation method. Add the solution dropwise to the (MoO3+WO3) / MgAl composite oxide, age at room temperature for 12 hours, vacuum dry for 12 hours, and calcine at 450℃ for 4 hours to obtain NiO-(MoO3+WO3) / MgAl composite oxide. Grind and mix the obtained NiO-(MoO3+WO3) / MgAl composite oxide with 0.19 g of potassium carbonate, calcine at 450℃ for 4 hours, and then perform sulfidation activation on the above product. The sulfidation gas is 10% H2S / H2 (space velocity 1000 h⁻¹). -1 The catalyst S-1 was obtained by sulfidation at a temperature of 400℃ and a sulfidation time of 2 hours.
[0082] The physicochemical properties of the catalyst are shown in Table 1. Among them, in catalyst S-1, based on the weight of the composite oxide support, the total amount of Mo and W elements is 6.5 wt%, the Ni element content is 2.1 wt%, and the K element content is 8.1 wt%.
[0083] Example 2 The method is the same as in Example 1, except that in step (2), the molar ratio of tetraethylammonium bromide (TEAB) to hexadecyltrimethylammonium bromide (CTAB) is 1:1. Catalyst S-2 is obtained.
[0084] The physicochemical properties of the catalysts are shown in Table 1. Specifically, in catalyst S-2, based on the weight of the composite oxide support, the total content of Mo and W is 6.4 wt%, the content of Ni is 2.2 wt%, and the content of K is 8.0 wt%.
[0085] Example 3 (1) The MgO-Al2O3 composite oxide support was obtained according to step (1) in Example 1.
[0086] (2) Prepare 6.47 mL of 0.22 M Na₂MoO₄ solution A and 2.16 mL of 0.22 M Na₂WO₄ solution B. While stirring, add 2.0 M HCl solution dropwise to adjust the pH of solutions A and B to 5. Then, add 12.6 mL of a pre-prepared 0.3 M tetraethylammonium bromide (TEAB) and hexadecyltrimethylammonium bromide (CTAB) with a molar ratio of 1:5 dropwise to solution A. Subsequently, add solution B to the above solution (molar ratio (CTAB+TEAB):(MoO₄) 2- +WO4 2- MoO4 = 2:1 2- :WO4 2-= 3:1), stirred for 2 hours to obtain a white emulsion suspension, then 1 g of the above MgO-Al2O3 composite oxide carrier was added, transferred to an autoclave, and subjected to hydrothermal deposition reaction at 120℃ for 24 hours. After cooling, the suspension was filtered, washed with water, dried at 120℃ for 10 hours, and calcined at 500℃ for 4 hours to obtain (MoO3+WO3) / MgAl composite oxide.
[0087] (3) Prepare an aqueous solution of nickel nitrate containing 0.14 g (approximately 0.75 mL), and load it by stepwise impregnation method. Add the solution dropwise to the (MoO3+WO3) / MgAl composite oxide, age at room temperature for 12 hours, vacuum dry for 12 hours, and calcine at 450℃ for 4 hours to obtain NiO-(MoO3+WO3) / MgAl composite oxide. Grind and mix the obtained NiO-(MoO3+WO3) / MgAl composite oxide with 0.19 g of potassium carbonate, calcine at 450℃ for 4 hours, and then perform sulfidation activation on the above product. The sulfidation gas is 10% H2S / H2 (space velocity 1000 h⁻¹). -1 The catalyst S-3 was obtained by sulfidation at 400℃ for 2 hours.
[0088] The physicochemical properties of the catalysts are shown in Table 1. Among them, in catalyst S-3, based on the weight of the composite oxide support, the total amount of Mo and W elements is 6.5 wt%, the content of Ni element is 2.0 wt%, and the content of K element is 8.2 wt%.
[0089] Example 4 The method in Example 1 is followed, except that in step (2), the molar ratio of CTAB and TEAB is 1:5, and the resulting catalyst is designated as S-4. The physicochemical properties of the catalyst are shown in Table 1. In catalyst S-4, based on the weight of the composite oxide support, the total amount of Mo and W elements is 6.4 wt%, the Ni element content is 2.1 wt%, and the K element content is 8.2 wt%.
[0090] Example 5 The method described in Example 1 is different, except that the MgAl composite oxide is prepared by a conventional co-precipitation method, specifically including: preparing a mixed alkaline solution with a NaOH concentration of 1.20 M at a molar ratio of n(NaOH):n(Na2CO3) = 8; preparing a nitrate (Mg(NO3)2·6H2O, Al(NO3)3·9H2O) solution with a total metal ion concentration of 0.60 M at a molar ratio of n(Mg):n(Al) = 7:3; adding the mixed alkaline solution to the mixed salt solution to adjust the pH to 8; aging the mixture by co-current precipitation and stirring at 65°C for 4 hours; cooling to room temperature; filtering; and washing with deionized water until neutral; drying the filter cake at 120°C for 12 hours; calcining at 500°C for 4 hours; and grinding into powder to obtain the MgO-Al2O3 composite oxide carrier.
[0091] The obtained catalyst is designated as S-5. The physicochemical properties of the catalyst are shown in Table 1. In catalyst S-5, based on the weight of the composite oxide support, the total content of Mo and W is 6.5 wt%, the content of Ni is 2.0 wt%, and the content of K is 8.4 wt%.
[0092] Example 6 Following the method in Example 1, except that CTAB was replaced with an equimolar amount of dodecyltrimethylammonium bromide, the resulting catalyst was designated S-6. The physicochemical properties of the catalyst are shown in Table 1. Specifically, in catalyst S-6, based on the weight of the composite oxide support, the total content of Mo and W elements was 6.3 wt%, the content of Ni element was 2.3 wt%, and the content of K element was 8.2 wt%.
[0093] Example 7 The method in Example 1 is followed, except that in step (1), the linear velocity of the liquid flow in the pores of the microchannel reactor is 0.1 m / s, and the resulting catalyst is designated as S-7. The physicochemical properties of the catalyst are shown in Table 1. In catalyst S-7, based on the weight of the composite oxide support, the total amount of Mo and W elements is 6.5 wt%, the Ni element content is 1.9 wt%, and the K element content is 8.4 wt%.
[0094] Example 8 The method was followed as in Example 1, except that the composite oxide support used was a MgO-Al2O3-TiO2 three-component composite oxide. Catalyst S-8 was obtained.
[0095] The specific preparation method includes: preparing a mixed alkaline solution with a NaOH concentration of 1.20 M at a molar ratio of n(NaOH):n(Na2CO3) = 8; and preparing a mixed salt solution (Mg(NO3)2·6H2O, Al(NO3)3·9H2O, TiCl4) with a total metal ion concentration of 0.60 M at a molar ratio of n(Mg):n(Al):n(Ti) = 7:3:1. The mixed alkaline solution is then added to the mixed salt solution to adjust the pH to 8. Under conditions of 65℃ and thorough stirring, the solution flows into a microchannel reactor. The linear velocity of the liquid flow within the channels of the microchannel reactor is 2 m / s. The channels of the microchannel reactor are rectangular, and the channel dimensions meet the following requirements: cross-sectional dimensions of 3 mm × 0.5 mm and a length of 800 mm. After the metal salt solution and alkaline solution are mixed in the microchannel, a uniform suspension is formed. After precipitation, stirring and aging continue for 4 hours. After cooling to room temperature, the solution is filtered and washed with deionized water until neutral. The filter cake was dried at 120℃ for 6 hours, then calcined at 500℃ for 4 hours, and ground into powder to obtain the MgO-Al2O3-TiO2 composite oxide carrier.
[0096] The physicochemical properties of the catalysts are shown in Table 1. Among them, in catalyst S-8, based on the weight of the composite oxide support, the total amount of Mo and W elements is 6.5 wt%, the Ni element content is 2.1 wt%, and the K element content is 8.1 wt%.
[0097] Comparative Example 1 Following the method in Example 1, except that the surfactant did not contain CTAB, the resulting catalyst was designated DS-1. The physicochemical properties of the catalyst are shown in Table 1. Specifically, in catalyst DS-1, based on the weight of the composite oxide support, the total content of Mo and W elements was 6.4 wt%, the content of Ni element was 2.2 wt%, and the content of K element was 8.2 wt%.
[0098] Comparative Example 2 Following the method in Example 5, except that the surfactant did not contain CTAB, the resulting catalyst was designated DS-2. The physicochemical properties of the catalyst are shown in Table 1. Specifically, in catalyst DS-2, based on the weight of the composite oxide support, the total content of Mo and W elements was 6.7 wt%, the content of Ni element was 2.0 wt%, and the content of K element was 8.4 wt%.
[0099] Comparative Example 3 (1) The MgO-Al2O3 composite oxide support was prepared according to the method in Example 1.
[0100] (2) Prepare 8.6 mL of 0.22 M Na₂MoO₄ solution A. While stirring, add 2.0 M HCl solution dropwise to adjust the pH of solution A to 5. Then, add 12.6 mL of a pre-prepared 0.15 M tetraethylammonium bromide (TEAB) and hexadecyltrimethylammonium bromide (CTAB) mixed solution with a molar ratio of 1:3 to solution A dropwise. The molar ratio is (CTAB+TEAB):MoO₄ 2- =1:1, stir for 2 hours to obtain a white emulsion suspension, then add 1 g of the above MgO-Al2O3 composite oxide support, transfer to a high pressure vessel, and carry out hydrothermal deposition reaction at 120℃ for 24 hours. After cooling, filter the suspension, wash with water, dry at 120℃ for 10 hours, and calcine at 500℃ for 4 hours to obtain MoO3 / MgAl composite oxide.
[0101] (3) Prepare an aqueous solution of nickel nitrate containing 0.14 g (approximately 0.75 mL), and load it onto the MoO3 / MgAl composite oxide using a stepwise impregnation method. Aging at room temperature for 12 hours, vacuum drying for 12 hours, and calcination at 450℃ for 4 hours yields the NiO-MoO3 / MgAl composite oxide. Grind and mix the obtained NiO-MoO3 / MgAl composite oxide with 0.19 g of potassium carbonate, and calcine at 450℃ for 4 hours to obtain the catalyst KNi,Mo / MgAl composite oxide. Activate the above product by sulfidation with 10% H2S / H2 (space velocity 1000 h⁻¹). -1 The catalyst DS-3 was obtained by vulcanizing at a temperature of 400℃ and a vulcanization time of 2 hours.
[0102] In catalyst DS-3, based on the weight of the composite oxide support, the content of Mo is 6.0 wt%, the content of Ni is 2.3 wt%, and the content of K is 8.8 wt%.
[0103] Table 1
[0104] Test case The catalytic performance of the catalysts used in the above examples and comparative examples for the production of ethanol and higher alcohols from syngas was evaluated. The reactions were carried out in a pressurized fixed-bed continuous flow reactor (ø11 mm) with a catalyst loading of 0.8 g. The sulfidated catalyst was directly switched to the reaction atmosphere. The reaction conditions were: 350 °C, 5.0 MPa, V(CO) / V(H2) / V(N2) = 45 / 45 / 10, GHSV = 2250 mL / g / h. Unreacted feedstocks and gaseous products were analyzed online using an SP7890 chromatograph with dual TCD and FID detectors. Alcohols and oxygen-containing compounds were analyzed using the internal standard method after absorption with isoamyl alcohol. The results are shown in Tables 2 and 3.
[0105] Table 2
[0106] Oxygen-containing compounds include alcohols, aldehydes, acids, and esters.
[0107] Table 3
[0108] Combining the results in Tables 1, 2, and 3, it can be seen that the average sheet length of the sulfide in the first metal component of the syngas-to-ethanol catalyst prepared in the embodiments of the present invention is small, and the matching degree between the average sheet length and the average number of layers is good. This indicates that the sulfide in the first metal component of the catalyst has good dispersibility, and when used in the reaction of syngas to produce ethanol and higher alcohols, it has a high conversion rate, high total alcohol selectivity, and good selectivity for lower alcohols. Under the synergistic effect of the composite surfactant, the active phase structure of the catalyst can be optimized by adjusting the type, amount, and ratio, thereby improving the final performance of the catalyst. A comparison between Examples 1 and 5 shows that the composite oxide support prepared by the microchannel method can further improve the dispersibility of the sulfide in the first metal component. A comparison between Examples 1 and 8 shows that the use of a three-component metal oxide can further improve the interaction between the active phases, thereby exhibiting a higher yield of the target product.
[0109] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for preparing a catalyst for syngas-to-methanol production, characterized in that, The preparation method includes: (1) Provide a solution A containing a molybdenum source and a solution B containing a tungsten source; the molar ratio of the molybdenum source to the tungsten source is 1-9:1, based on elemental composition. The pH values of solutions A and B are each independently selected from 1 to 6; (2) Under stirring conditions, a surfactant and solution B are introduced into solution A to obtain a mixture; The surfactant comprises a first surfactant and a second surfactant; the first surfactant is selected from C6-C10 alkyl quaternary ammonium salts, and the second surfactant is selected from C12-C20 alkyl quaternary ammonium salts; the molar ratio of the second surfactant to the first surfactant is 1-3:1; (3) The above mixture is mixed with the composite oxide carrier, hydrothermal deposition is performed, and then a first calcination is performed to obtain the first precursor; The composite oxide support was prepared by co-precipitation in microchannels; (4) The second metal component and the third metal component are loaded onto the first precursor; the second metal component is selected from at least one transition metal other than molybdenum and tungsten; the third metal component is selected from at least one alkali metal. (5) The product obtained in step (4) is activated by sulfurization.
2. The preparation method according to claim 1, wherein, In step (1), the pH of solution A and solution B are each independently selected from 2 to 4.
3. The preparation method according to claim 1, wherein, In step (1), the pH of solutions A and B is adjusted by introducing inorganic acids.
4. The preparation method according to claim 3, wherein, The inorganic acid is hydrochloric acid and / or nitric acid.
5. The preparation method according to claim 1, wherein, The molybdenum source is selected from molybdenum-containing soluble salts; And / or, the tungsten source is selected from tungsten-containing soluble salts.
6. The preparation method according to claim 5, wherein, The molybdenum source is sodium molybdate and / or ammonium molybdate; And / or, the tungsten source is sodium tungstate and / or ammonium tungstate.
7. The preparation method according to claim 1, wherein, The molar ratio of molybdenum source to tungsten source is 1-6:1, based on elemental composition.
8. The preparation method according to any one of claims 1-3, wherein, In step (2), the molar ratio of the amount of surfactant to the total amount of tungsten source and molybdenum source (in terms of elements) is 0.2-10:1; And / or, the first surfactant is tetraethylammonium bromide and the second surfactant is hexadecyltrimethylammonium bromide.
9. The preparation method according to claim 8, wherein, In step (2), the molar ratio of the amount of surfactant to the total amount of tungsten source and molybdenum source (in terms of elements) is 1-2:
1.
10. The preparation method according to any one of claims 1-3, wherein, In step (3), based on the weight of the composite oxide support, the total amount of the molybdenum source and tungsten source used is 2-50 wt% (calculated by molybdenum and tungsten elements). And / or, the conditions for the hydrothermal deposition include: a reaction temperature of 80-160°C and a reaction time of 5-36 h.
11. The preparation method according to claim 10, wherein, In step (3), based on the weight of the composite oxide carrier, the total amount of the molybdenum source and tungsten source used is 6-20 wt% (calculated by molybdenum and tungsten elements). And / or, the conditions for the hydrothermal deposition include: a reaction temperature of 80-120°C and a reaction time of 16-30 h.
12. The preparation method according to any one of claims 1-3, wherein, Step (4) includes: (4-1) The second metal component is loaded onto the first precursor by an impregnation method; (4-2) The product obtained in step (4-1) is mixed with the salt of the third metal component to obtain the second precursor.
13. The preparation method according to any one of claims 1-3, wherein, Based on the weight of the composite oxide carrier, the amount of the second metal component is 2-20 wt% (elementally). The amount of the third metal component is 1-12 wt%; And / or, elementally, the molar ratio of the second metal component to the total amount of molybdenum source and tungsten source is 0.2-2.5:1; And / or, in terms of elements, the molar ratio of the third metal component to the total amount of molybdenum source and tungsten source is 0.1-4:1; And / or, the second metal component is selected from at least one of Ni, Co, Mn and Rh; And / or, the third metal component is Na and / or K.
14. The preparation method according to claim 13, wherein, Based on the weight of the composite oxide carrier, the amount of the second metal component is 2-10 wt% (elementally). The amount of the third metal component is 2-10 wt%; And / or, elementally, the molar ratio of the second metal component to the total amount of molybdenum source and tungsten source is 0.5-1.5:1; And / or, in terms of elements, the molar ratio of the third metal component to the total amount of molybdenum source and tungsten source is 0.5-4:1; And / or, the second metal component is Ni.
15. The preparation method according to any one of claims 1-3, wherein, In step (5), the sulfurization activation includes contacting the product obtained in step (4) with sulfur gas.
16. The preparation method according to claim 15, wherein, The conditions for sulfurization activation include: a temperature of 300-600℃ and a time of 2-10 hours; and a volume hourly space velocity (VHSV) of 200-4000 h⁻¹ for the sulfurizing gas. -1 .
17. The preparation method according to claim 16, wherein, The conditions for sulfurization activation include: a temperature of 350-450℃ and a time of 2-4 hours.
18. The preparation method according to claim 15, wherein, The sulfiding gas is a mixture of H2S, H2, and optionally an inert gas.
19. The preparation method according to claim 18, wherein, The sulfurized gas contains 10-20% H2S by volume and 80-90% H2 by volume.
20. The preparation method according to any one of claims 1-3, wherein, The composite oxide support is a two-component or three-component composite oxide support. The two-component composite oxide support is selected from at least one of MgO-Al2O3, CaO-Al2O3, TiO2-CaO, Al2O3-ZrO2, TiO2-MgO, TiO2-Al2O3, MgO-SiO2, Al2O3-SiO2 and MgO-ZrO2. The three-component composite oxide support is TiO2-MgO-Al2O3 and / or ZrO2-MgO-Al2O3.
21. The preparation method according to any one of claims 1-3, wherein, The preparation method of the composite oxide support includes: S1. A solution containing soluble compounds and a precipitant solution of the composite components are fed into a microchannel reactor in parallel to carry out a precipitation reaction within the microchannel. S2. The product obtained from the above precipitation reaction is aged, dried and calcined.
22. The preparation method according to claim 21, wherein, The conditions for the precipitation reaction include: precipitation temperature of 10-80℃ and pH of 6-10; And / or, the linear velocity of the liquid flow within the pores of the microchannel reactor is not less than 0.05 m / s.
23. The preparation method according to claim 22, wherein, The conditions for the precipitation reaction include: precipitation temperature of 20-65℃ and pH of 7-9; And / or, the linear velocity of the liquid flow within the pores of the microchannel reactor is not less than 0.1 m / s.
24. A syngas-to-methanol catalyst prepared by the preparation method according to any one of claims 1-23.
25. The application of the syngas-to-methanol catalyst according to claim 24 in the syngas-to-methanol reaction.
26. A method for producing ethanol and higher alcohols from syngas, the method comprising: Under the conditions of syngas-to-methanol reaction, syngas is brought into contact with a catalyst; The catalyst is the syngas-to-methanol catalyst according to claim 24.
27. The method according to claim 26, wherein, The reaction conditions for syngas-to-methanol production include: a reaction temperature of 250-400℃, a reaction pressure of 2-8MPa, and a syngas space velocity of 1000-5000 mL / g / h. And / or, in the synthesis gas, the volume ratio of CO to H2 is 0.5-1:1.
Citation Information
Patent Citations
Catalyst for synthesis of gas produced low-carbon mixed alcohol and production method thereof
CN101428229A
Cobalt-nickel-molybdenum-potassium (Co-Ni-Mo-K) catalyst for preparing low carbon alcohol by synthetic gas and preparation method thereof
CN102125857A
Preparation method and application of molybdenum sulfide catalyst using SBA-15 as carrier for producing low-carbon alcohols from synthetic gas
CN102351641A
Carbon-supported catalysts for production of higher alcohols from syngas
CN103313785A
Catalyst for preparing mixing alcohol with low carbon from synthesis gas and its preparing method
CN1431049A