Titanium ball automatic implantation laser cladding method, device and readable storage medium
By using AOB laser welding equipment and a spiral path combined with protective gas, the problems of porosity and embrittlement in titanium alloy welding have been solved, achieving high-quality welding results and improving welding efficiency and plasticity.
Patent Information
- Application Number
- CN202410390132.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-29
AI Technical Summary
In existing titanium alloy laser welding processes, nitrogen, oxygen, and hydrogen from the air are easily absorbed, forming interstitial solid solutions. This leads to embrittlement and poor plasticity of the weld, and also easily forms pores.
Using AOB laser welding equipment, a spiral path is set from the inside out through a combination of inner and outer core laser beams. Combined with a protective gas, the laser welding speed and power are controlled to prevent the welding material from reacting with the air and forming pores.
It improves welding quality, reduces spatter and porosity, enhances welding stability and plasticity, and improves welding efficiency and wear resistance.
Smart Images

Figure CN118046085B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of laser cladding technology, and in particular to a method, apparatus, and readable storage medium for automatic titanium ball placement and laser cladding. Background Technology
[0002] Currently, titanium alloys are the main material used for mobile phone frames and buttons. Titanium alloys have many advantages, such as low density, high strength, good plasticity and toughness, good machinability, and good heat and corrosion resistance. Therefore, they have been widely used in mobile phone manufacturing, enabling mobile phones to be lighter and stronger.
[0003] However, in existing welding methods, due to the extreme temperature gradient inside the molten pool during the welding process, the gas trapped in the molten pool does not have time to escape after the weld pool solidifies rapidly, thus forming pores at the bottom of the molten pool.
[0004] Existing titanium alloy laser welding readily absorbs nitrogen, oxygen, and hydrogen from the surrounding air and reacts with them to form interstitial solid solutions. This hinders the movement of intergranular dislocations, significantly increasing the hardness of the weld, but reducing its plasticity and causing the entire weld joint to become brittle. Summary of the Invention
[0005] In view of this, the purpose of this invention is to overcome the shortcomings of the prior art and provide a method, apparatus and readable storage medium for automatic titanium ball laser cladding.
[0006] In a first aspect, the present invention provides a laser cladding method, comprising:
[0007] Obtain the Z-axis corresponding to the laser focal point of the laser cladding device;
[0008] Determine the laser cladding path based on the welding material parameters;
[0009] The laser welding speed, laser output power, and ball ejection time are determined based on the laser cladding path.
[0010] The laser cladding device welds the welding material according to the laser cladding path, the laser welding speed, and the output power of the laser.
[0011] Material cutting and cladding welding completed.
[0012] Furthermore, the output power of the laser includes the output power of the outer core of the laser and the output power of the inner core of the laser.
[0013] Furthermore, the laser cladding method also includes: determining whether there is a deviation at the welding point;
[0014] If so, then reset the welding points.
[0015] Furthermore, the laser cladding path is a spiral path from the inside out.
[0016] Further, after the step of determining the laser welding speed and the laser output power based on the laser cladding path, the process includes:
[0017] The ball-planting mechanism is set up for automatic feeding.
[0018] Furthermore, the ball release time is t, where the value of t ranges from 10ms to 20ms.
[0019] Furthermore, the laser welding speed is v, where the value of v ranges from 400 mm / s to 600 mm / s.
[0020] In a second aspect, the present invention provides a laser cladding apparatus, the laser cladding apparatus comprising: a laser, an automatic titanium ball conveying mechanism, a memory, a processor, and a laser cladding program stored in the memory and running on the processor, wherein the laser cladding program, when executed by the processor, implements the steps of the laser cladding method.
[0021] Thirdly, the present invention provides a computer-readable storage medium storing a laser cladding program, which, when executed by a processor, implements the steps of the laser cladding method as described above.
[0022] The embodiments of the present invention have the following advantages: The laser cladding method provided in this application can reduce the high temperature vaporization of the central material and the generation of metal gas during the processing by changing the energy distribution of the laser spot, and can also effectively suppress the spatter generated during the welding process and avoid the formation of pores.
[0023] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, preferred embodiments are described below in detail with reference to the accompanying drawings. Attached Figure Description
[0024] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 A flowchart of an automated titanium ball laser cladding method according to some embodiments of the present invention is shown;
[0026] Figure 2 The present invention provides a flowchart of a method for determining the welding point in an automatic titanium ball placement laser cladding method according to some embodiments of the present invention;
[0027] Figure 3 The present invention provides an automatic titanium ball laser cladding method for titanium ball placement, and describes the appearance of the titanium balls after welding and melting, according to some embodiments of the present invention.
[0028] Figure 4 The following are metallographic cross-sectional views of titanium balls after welding, provided by some embodiments of the present invention, regarding an automatic titanium ball placement and laser cladding method. Detailed Implementation
[0029] Embodiments of the present invention are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0030] It should be noted that when an element is said to be "fixed" to another element, it can be directly on the other element or there may be an intervening element. When an element is said to be "connected" to another element, it can be directly connected to the other element or there may be an intervening element. Conversely, when an element is said to be "directly" on another element, there is no intervening element. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.
[0031] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0032] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.
[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein in the template description is for the purpose of describing particular embodiments only and is not intended to limit the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0034] like Figure 1 As shown, some embodiments of the present invention provide an automatic titanium ball laser cladding method, which is mainly applied to the welding cladding of materials used in mobile phone frames and mobile phone buttons. This method avoids the formation of vacuum pores in the welding material during the welding process, thereby improving the welding quality.
[0035] Specifically, laser cladding methods include:
[0036] Step S100: Obtain the Z-axis corresponding to the laser focus of the laser cladding device.
[0037] In this embodiment, the laser cladding device is an AOB laser welding device, which is composed of a 4000W laser inner core and a 4000W laser outer core. The inner core has a diameter of 50μm and the outer core has a diameter of 150μm. It can realize real-time output power feedback and power closed-loop compensation, and the output spot of the laser can be freely adjusted according to the processing requirements.
[0038] It should be noted that AOB laser welding equipment has a large outer core diameter, which can increase the weld width and thus improve the tolerance for weld gaps.
[0039] Meanwhile, the outer core diameter of the AOB laser welding equipment has a preheating effect, which can ensure the aesthetic appearance of the weld.
[0040] Secondly, AOB laser welding equipment has a small core diameter and a high power output, which can ensure the weld penetration depth.
[0041] By simultaneously welding the inner and outer cores at two stations, the loading, clamping, welding, and unloading times can be saved, thus improving the welding efficiency of the welding station.
[0042] Specifically, adjust the laser head of the laser cladding device to make light-emitting dots in the Z-axis direction (here, the Z-axis refers to the vertical direction), determine the position of the laser focal point of the laser in the laser cladding device, and determine the Z-axis corresponding to the laser focal point in the laser's output direction based on the laser focal point.
[0043] It should be noted that this AOB welding equipment uses water cooling, which can improve heat dissipation efficiency, ensure the stability of the laser head during the welding process, and thus ensure welding quality.
[0044] Step S200: Determine the laser cladding path based on the welding material parameters.
[0045] The welding materials include titanium balls, titanium plates, and aluminum plates, with the aluminum plates and titanium plates stacked together. The aluminum plates have mounting holes for accommodating the titanium balls.
[0046] It should be noted that the welding material parameters include the diameter of the titanium ball and the diameter of the mounting hole.
[0047] Specifically, the titanium ball is placed in the mounting hole, so that the outer wall of the titanium ball in the mounting hole fits against the wall of the mounting hole.
[0048] In this embodiment, the diameter of the titanium ball is larger than the diameter of the mounting hole, so that when the titanium ball is placed in the mounting hole, the edge of the titanium ball can fit against the opening edge of the mounting hole. The laser cladding path is set according to the fit position between the titanium ball and the hole wall.
[0049] It should be noted that, in this embodiment, the laser cladding path is a spiral path from the inside out. That is, the connection between the titanium ball and the aluminum plate is welded and clad in a spiral shape from the vertical axis of the titanium ball outwards.
[0050] It is understandable that by using a spiral welding path from the inside out, the side of the titanium ball facing the aluminum hole can be connected to the aluminum plate to prevent the titanium ball from shifting in the aluminum hole during the welding process. This ensures that the vertical axis of the titanium ball always coincides with the axis of the aluminum hole during the welding process, thereby improving the welding quality.
[0051] In addition, by setting a spiral welding path from the inside out, not only can the stability of the welding process be improved, but welding gaps can also be effectively avoided during laser welding cladding, thereby improving the continuity and quality of the welding.
[0052] Step S300: Determine the laser welding speed and laser output power based on the laser cladding path.
[0053] Specifically, in this embodiment, the laser welding speed is v, where the value of v ranges from 400 mm / s to 600 mm / s. It can be understood that the laser welding speed can be any value between 400 mm / s and 600 mm / s, and can be specifically set according to actual conditions.
[0054] In addition, by adjusting the protective gas pressure, the oxidation reaction between the welding material and oxygen in the air can be avoided during the laser welding process, thereby ensuring the welding quality of the welding material.
[0055] In step S400, the laser cladding device welds the welding material according to the laser cladding path, the laser welding speed, and the laser output power.
[0056] By placing the welding material at the welding station of the laser cladding device, starting the laser cladding device, and welding the welding material according to the set laser cladding path, laser welding speed, and laser output power.
[0057] It should be noted that during the welding process, a protective gas is sprayed onto the titanium ball through the jet head in the laser cladding device. This protective gas is used to expel the air around the titanium ball, thereby forming a protective gas around the titanium ball. This prevents the titanium ball from reacting with gases such as oxygen and nitrogen in the air during the laser cladding welding process, thus forming a gas protective layer around the titanium ball and improving the quality of laser cladding welding.
[0058] Step S500: Unload the material and complete the cladding welding.
[0059] Specifically, the welding material is removed from the laser cladding device to complete the cladding welding of the welding material.
[0060] The laser cladding method provided in this application changes the energy distribution of the laser spot, that is, sets the laser beam into a ring beam and a central beam. This not only reduces the high temperature vaporization of the central material and the generation of metal gas during the processing, but also effectively suppresses spatter generated during the welding process and avoids porosity.
[0061] It should be noted that the ring beam refers to the beam emitted from the outer core of the laser welding device, while the center beam refers to the beam emitted from the inner core of the laser welding device.
[0062] In this embodiment, the radius of the spiral point of the laser welding is r, where the value of r is in the range of 0.9mm≤r≤1mm, and can be set according to the actual situation.
[0063] For example, in this embodiment, a titanium ball with a diameter of 3mm is used as the welding material, an aluminum plate with a thickness of 2mm is used, an aluminum hole with a diameter of 2.85mm is opened in the thickness direction of the aluminum plate, and a titanium plate with a thickness of 1mm is used as the base plate, and the titanium ball is placed in the aluminum hole.
[0064] The laser welding path was set to a spiral point with a radius of 0.95 mm (helical welding from the inside out), the welding speed was 550 mm / s, the laser power was set to 1680 W for the inner core and 1720 W for the outer core. The laser focus was positively defocused at 2, and a protective gas (argon) was continuously blown during the welding process.
[0065] Specifically, the welding penetration depth obtained by the laser cladding method provided in this application can reach 0.77 mm, with not only small gaps at the weld edges, but also almost no pores inside.
[0066] Due to the high density of laser focal points, welding at the laser focal point can easily result in spatter and other issues.
[0067] Based on this, in some embodiments of the present invention, the laser focus is set to positive defocus of 2. It should be noted that positive defocus means that the distance between the welding head and the workpiece is greater than the minimum focusing diameter of the welding head.
[0068] In this state, the weld head diameter increases, the welding power density decreases, but the welding energy distribution is more uniform, increasing the tolerance of the welding process. Positive defocusing is suitable for welding thick plates, highly reflective metals, and porous materials.
[0069] Understandably, by setting the laser focus to positive defocus to avoid spatter during welding, not only can the stability and safety of the welding process be guaranteed, but the welding quality can also be improved.
[0070] In this embodiment, by setting an inner core and an outer core of the laser, the laser beam shape can be adjusted according to the actual situation. By using power combining of the inner core and the outer core, the ratio between the power of the inner core and the power of the outer core can be flexibly and independently adjusted. This allows the laser cladding method provided by the present invention to adapt to more processing scenarios, thereby meeting the processing needs of different welding materials and improving welding efficiency.
[0071] Understandably, the laser cladding method provided in this application improves the quality, saves costs, and increases efficiency in the production of mobile phone buttons made of titanium alloy materials, and significantly improves the wear resistance of titanium alloys.
[0072] In addition, in some embodiments of the present invention, the welding process of the welding material by the laser cladding equipment also includes blowing protective gas onto the surface of the titanium ball, so that the protective gas forms a protective effect around the titanium ball, avoiding spatter during the welding process, and preventing the welding part of the welding material from reacting with oxygen, nitrogen, hydrogen and other gases in the air to form interstitial solid solutions, thereby ensuring the quality of welding cladding.
[0073] Specifically, the protective gas is an inert gas.
[0074] In some embodiments of the present invention, a trial run of the laser cladding device is performed before welding the welding materials.
[0075] The trial operation of the laser cladding device was conducted to confirm whether the device could operate normally and whether the welding points were accurate, thereby ensuring the stability and quality of the welding process.
[0076] In some embodiments of the present invention, the laser cladding method further includes an automatic feeding mechanism for ball placement. Specifically, the welding material is placed at the welding position of the laser cladding device, such that the welding point of the welding material is directly opposite the laser of the laser cladding device.
[0077] Additionally, it should be noted that in some embodiments of the present invention, the ball release time is t, where the value of t ranges from 10ms to 20ms. It is understood that the ball release time can be any value between 10ms and 20ms, and can be specifically set according to the actual situation.
[0078] It should be noted that the ball ejection time refers to the time it takes for the welding material to be ejected from the start of welding to the completion of welding, in order to achieve continuous welding of the welding material and improve the welding efficiency.
[0079] In some embodiments of the present invention, the output power of the laser includes the output power based on the outer core diameter of the laser and the output power based on the inner core diameter of the laser.
[0080] Understandably, by separately setting the power of the outer core diameter and the output power of the inner core diameter of the laser, the power of the inner ring and the power of the outer ring can be controlled separately, thereby forming a combined ring beam and a central beam. This allows for control over different welding application scenarios to achieve the best welding effect, avoid spatter or even porosity during the welding process, and improve welding quality.
[0081] like Figure 2 As shown, in some embodiments of the present invention, the automatic titanium ball laser cladding method further includes:
[0082] Step S110: Determine whether there is a deviation in the welding point position.
[0083] Specifically, after step S300, the automatic welding program of the laser cladding device is tested. During the test welding process, the welding points of the laser are checked for any deviations.
[0084] Step S111: If yes, then reset the welding point position.
[0085] Specifically, if welding point deviations occur during trial operation, the laser cladding equipment needs to be reset and nine-point correction performed.
[0086] If not, proceed to step S112. If not, proceed to step S400.
[0087] Understandably, if there is no deviation in the welding point, it means that the laser cladding device is operating normally, that is, the laser welding point is accurate.
[0088] It should be noted that, Figure 3 This image shows the appearance of the titanium ball under a microscope after welding and melting. As can be seen from the image, the surface is smooth and flat under the microscope, with almost no spatter. Furthermore, Figure 4 After metallographic corrosion, the cross-section observed under a microscope has very small pores, almost no pores, and the edges are closely fitted, indicating a certain melting depth.
[0089] Other embodiments of the present invention provide a laser cladding apparatus, the laser cladding apparatus comprising: a titanium ball conveying mechanism for conveying titanium balls to a working position. The laser cladding apparatus further comprises a laser, a processor, and a laser cladding program stored in the memory and running on the processor, the laser cladding program, when executed by the processor, implementing the steps of the laser cladding method as described in any of the foregoing embodiments.
[0090] When the laser cladding program running on the laser cladding device is executed, the method implemented can be referred to in the various embodiments of the laser cladding method in this invention, and will not be repeated here.
[0091] Some embodiments of the present invention provide a computer-readable storage medium storing a laser cladding program, which, when executed by a processor, implements the steps of the laser cladding method as described in any of the above embodiments.
[0092] In all examples shown and described herein, any specific values should be interpreted as merely exemplary and not as limitations; therefore, other examples of exemplary embodiments may have different values.
[0093] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0094] The above-described embodiments are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention.
Claims
1. A method for automatic implantation of titanium ball by laser cladding, characterized in that, include: Obtain the Z-axis corresponding to the laser focal point of the laser cladding device; The laser cladding path is determined based on the welding material parameters. The laser cladding path is a spiral path from the inside to the outside. The welding material includes titanium balls, titanium plates, and aluminum plates. The aluminum plates and titanium plates are stacked together. The aluminum plates have mounting holes for accommodating the titanium balls. The laser welding speed, laser output power, and ball ejection time are determined based on the laser cladding path. The laser output power includes the output power of the outer core of the laser and the output power of the inner core of the laser. The laser cladding device welds the material according to the laser cladding path, the laser welding speed, and the output power of the laser. The radius of the spiral point of the laser welding is r, where the value of r is in the range of 0.9mm≤r≤1mm. The laser welding speed is v, where the value of v ranges from 400 mm / s to 600 mm / s; the ball ejection time is t, where the value of t ranges from 10 ms to 20 ms. Material cutting and cladding welding completed.
2. The automatic titanium ball implantation laser cladding method according to claim 1, characterized in that, The laser cladding method further includes: determining whether there is a deviation in the welding point; If so, then reset the welding points.
3. The automatic titanium ball implantation laser cladding method according to claim 1, characterized in that, After determining the laser welding speed and laser output power based on the laser cladding path, the process includes: The ball-planting mechanism is set up for automatic feeding.
4. A laser cladding device, characterized in that, The laser cladding apparatus includes: a laser, an automatic titanium ball conveying mechanism, a memory, a processor, and a laser cladding program stored in the memory and running on the processor. When the laser cladding program is executed by the processor, it implements the steps of the laser cladding method as described in any one of claims 1 to 3.
5. A computer-readable storage medium, characterized in that, The computer-readable storage medium stores a laser cladding program, which, when executed by a processor, implements the steps of the laser cladding method as described in any one of claims 1 to 3.
Citation Information
Patent Citations
Laser cladding method and device and computer readable storage medium
CN111428341A
In-light coaxial ball feeding laser cladding head and cladding system
CN211079337U