A method for producing an interlocked polyurethane material and an interlocked polyurethane-polyimide material
By introducing metal coordination bonds into polyurethane and polyimide networks to form interlocking structures, the problem of insufficient thermal and mechanical properties of polyurethane materials is solved, and high-strength and high-toughness polymer materials are prepared.
Patent Information
- Application Number
- CN202410184218.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-19
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-19
AI Technical Summary
Existing polyurethane materials have shortcomings in terms of thermal and mechanical properties, making it difficult to simultaneously achieve high strength and high toughness. Traditional dual-network materials also suffer from poor performance due to problems such as thermodynamic incompatibility and phase separation.
The cross-linked polyurethane and polyimide networks are interlocked by metal coordination bonds. The organic cuprous ion Cu(I) forms metal coordination bonds with the N atoms on the phenanthroline diphenylamine and polyimide chains, thereby realizing non-covalent interaction between the polymer chains and forming an "interlocked" structure.
The prepared interlocking polyurethane-polyimide material exhibits excellent mechanical and thermal properties, filling the gaps in strength and toughness of traditional materials, and possesses high mechanical properties and high heat resistance.
Smart Images

Figure CN118047929B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer material preparation technology, and in particular to an interlocking polyurethane material and a method for preparing an interlocking polyurethane-polyimide material. Background Technology
[0002] In recent years, global demand for polymer materials has been increasing, and commercial polymer materials are influencing and changing our lives. Whether in construction, clothing, vehicles, or food packaging, these polymer materials are ubiquitous in our daily lives.
[0003] Polyurethane (PU), as a new type of polymer material, has attracted much attention due to its excellent comprehensive properties, recyclability and broad application prospects. It has a wide range of applications in aerospace, automotive, textile, construction, medical, and intelligent detection fields.
[0004] Polyimide (PI) is an aromatic heterocyclic polymer compound with imide chain segments in its molecular structure. It is one of the most heat-resistant engineering plastics currently available and is widely used in aerospace, microelectronics, nanotechnology, liquid crystals, lasers, and other fields. Due to its outstanding performance and synthesis characteristics, PI has enormous application prospects as both a structural and functional material and is hailed as the pinnacle of polymer materials.
[0005] Significantly improving the preparation technology of traditional materials and developing polymer materials with exceptional mechanical properties is of great scientific importance. Modern society and industry urgently need to develop polymer materials with excellent mechanical properties and diverse functions. Combining polyimide with polyurethane materials holds promise for effectively solving the problem of simultaneously achieving both strength and toughness; interpenetrating networks or double networks offer an effective solution.
[0006] Existing polyurethane materials generally suffer from poor thermal and mechanical properties, which need further improvement.
[0007] Meanwhile, interpenetrating networks or dual-networks are developed by integrating two or more independent cross-linked networks. Over the past decade, interpenetrating network or dual-network polymers have attracted considerable interest from scientists due to their structural characteristics, leading to the creation of new networks or the improvement of their mechanical properties. Traditionally, dual-network polymer blending, which involves mixing two or more polymers with different structures and properties to achieve a blend with good overall performance by combining their strengths and weaknesses, is a commonly used polymer composite method. However, due to thermodynamic incompatibility, phase separation, and other issues, traditional dual-network materials do not offer superior performance (thermal and mechanical properties). Summary of the Invention
[0008] In view of this, the purpose of this invention is to provide an interlocking polyurethane material and a method for preparing an interlocking polyurethane-polyimide material. The interlocking polyurethane material and interlocking polyurethane-polyimide material prepared by the method provided by this invention have excellent mechanical and thermal properties.
[0009] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0010] This invention provides a method for preparing an interlocking polyurethane material, comprising the following steps:
[0011] Polyester diol, isocyanate monomer and catalyst are dissolved and mixed, and a nucleophilic addition reaction is carried out to obtain polyurethane prepolymer;
[0012] The polyurethane prepolymer, aliphatic diamine, and phenanthroline diphenylamine are dissolved and mixed, and then subjected to a polymerization reaction to obtain a cross-linked polyurethane.
[0013] The cross-linked polyurethane and organic cuprous oxide are dissolved and mixed to carry out a first coordination reaction, thereby obtaining the interlocked polyurethane material.
[0014] Preferably, the polyester diol comprises polycarbonate diol and / or polycaprolactone diol; the molecular weight of the polyester diol is 1000 to 4000.
[0015] The isocyanate monomer includes one or more of isophorone diisocyanate, toluene diisocyanate and hexamethylene diisocyanate;
[0016] The molar ratio of the polyester diol to the isocyanate monomer is 1:1 to 5.
[0017] Preferably, the catalyst comprises dibutyltin dilaurate;
[0018] The molar ratio of the catalyst to the isocyanate monomer is 0.009 to 0.1:1.
[0019] Preferably, the nucleophilic addition reaction is carried out at a temperature of 60–90°C for a time of 2–6 hours.
[0020] Preferably, the aliphatic diamine comprises one or more of 4,4'-diaminodicyclohexylmethane, methylcyclohexanediamine, and ethylenediamine;
[0021] The phenanthroline diphenylamine includes 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine;
[0022] The molar ratio of the aliphatic diamine to phenanthroline diphenylamine is 1:0.2 to 1;
[0023] The molar ratio of the fatty diamine to the isocyanate monomer is 1:1 to 5.
[0024] Preferably, the polymerization reaction is carried out at a temperature of 50–80°C for 2–5 hours.
[0025] Preferably, the organic cuprous oxide comprises tetraethyl copper tetrafluoroborate; the molar ratio of the organic cuprous oxide to phenanthrene diphenylamine is 0.1–1:0.2–1.
[0026] Preferably, the temperature of the first coordination reaction is 40–80°C and the time is 3–5 h.
[0027] This invention also provides a method for preparing an interlocking polyurethane-polyimide material, comprising the following steps:
[0028] Crosslinked polyurethane was prepared according to the preparation method described in the above technical solution;
[0029] The cross-linked polyurethane, polyimide and organic cuprous oxide are dissolved and mixed, and a second coordination reaction is carried out to obtain the interlocked polyurethane-polyimide material.
[0030] The polyimide is obtained by sequentially acylation and imidization of 4,4'-oxybisphthalic anhydride and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine.
[0031] Preferably, the organic cuprous oxide is tetraethyl copper tetrafluoroborate;
[0032] The molar ratio of phenanthroline diphenylamine in the crosslinked polyurethane to 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine in the polyimide is 0.1-1:0.1-1;
[0033] The ratio of the total amount of phenanthroline diphenylamine in the crosslinked polyurethane and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine in the polyimide to the amount of organic cuprous oxide is 0.2-1:0.15-1.
[0034] The second coordination reaction is carried out at a temperature of 40–80°C for 3–5 hours.
[0035] This invention provides a method for preparing an interlocking polyurethane material, comprising the following steps: dissolving and mixing polyester diol, isocyanate monomer and catalyst, and carrying out a nucleophilic addition reaction to obtain a polyurethane prepolymer; dissolving and mixing the polyurethane prepolymer, aliphatic diamine and phenanthroline diphenylamine, and carrying out a polymerization reaction to obtain a crosslinked polyurethane; dissolving and mixing the crosslinked polyurethane and organic cuprous oxide, and carrying out a first coordination reaction to obtain the interlocking polyurethane material.
[0036] This invention approaches the problem from the perspective of network structure design, crosslinking and entangled the structural units in crosslinked polyurethane through the action of metal coordination bonds. Due to their reversible nature, metal coordination bonds have the function of dynamic bond recombination and exchange, which can achieve dynamic "interlocking", ultimately giving the polyurethane material a significant improvement in mechanical and thermal properties.
[0037] This invention also provides a method for preparing an interlocking polyurethane-polyimide material, comprising the following steps: preparing a cross-linked polyurethane according to the preparation method described above; dissolving and mixing the cross-linked polyurethane, polyimide, and organic cuprous oxide, and performing a second coordination reaction to obtain the interlocking polyurethane-polyimide material; wherein the polyimide is obtained by sequentially acylation and imidization treatment of 4,4'-oxybisphthalic anhydride and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine.
[0038] In this invention, a dual-network structure (a rigid polyimide network and a flexible polyurethane network) is constructed. The monovalent copper ions Cu(I) in the organic cuprous oxide form a metal-ligand coordination interaction with the nitrogen atom on 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine in the polyimide network. This interaction, known as the metal-coordinate bond Cu(I)-4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine, connects two completely independent polymer chains through a non-covalent interaction, achieving a theoretical "interlocking" between the polymer chains. Unlike traditional single polymer networks or dual-network structures, this "interlocking" structure ingeniously combines rigid polyimide chains and flexible polyurethane chains for the first time. Based on interpenetrating polymer networks, this invention utilizes the metal ions Cu(I) from organic cuprous oxide to coordinate with phenanthroline diphenylamine on the polyurethane chain and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine on the polyimide chain, respectively, forming metal coordination bonds with Cu(I) as the corresponding coordination center ion. Thanks to the combination of the rigid and flexible polyurethane and polyimide chains, and the successful introduction of metal coordination bonds, the interlocking polyurethane-polyimide material prepared by this invention exhibits unique interlocking structural characteristics and outstanding mechanical properties. The interlocking polyurethane-polyimide material prepared by this invention effectively fills the gap in strong, tough, and functionally diverse polymer materials, improving upon the common problems of traditional polymer materials being strong yet brittle, or soft yet flexible. It is of great significance for developing polymer materials with high mechanical properties and high heat resistance. Attached Figure Description
[0039] Figure 1 Infrared spectra of the interlocking materials obtained in Examples 1-4;
[0040] Figure 2The XRD curves of the interlocking materials obtained in Examples 1-4 are shown.
[0041] Figure 3 The stress-strain curves of the interlocking materials obtained in Examples 1-4 are shown.
[0042] Figure 4 A schematic diagram of the polyurethane-polyimide "interlocking" structure;
[0043] Figure 5 This is a schematic diagram of the thermogravimetric curves of the interlocking materials obtained in Examples 1-4. Detailed Implementation
[0044] This invention provides a method for preparing an interlocking polyurethane material, comprising the following steps:
[0045] Polyester diol, isocyanate monomer and catalyst are dissolved and mixed, and a nucleophilic addition reaction is carried out to obtain polyurethane prepolymer;
[0046] The polyurethane prepolymer, aliphatic diamine, and phenanthroline diphenylamine are dissolved and mixed, and then subjected to a polymerization reaction to obtain a cross-linked polyurethane.
[0047] The cross-linked polyurethane and organic cuprous oxide are dissolved and mixed to carry out a first coordination reaction, thereby obtaining the interlocked polyurethane material.
[0048] Unless otherwise specified, all raw materials used in this invention are preferably commercially available products.
[0049] This invention involves dissolving and mixing polyester glycol, isocyanate monomer, and catalyst to carry out a nucleophilic addition reaction, thereby obtaining a polyurethane prepolymer.
[0050] In this invention, the polyester diol preferably comprises polycarbonate diol (PCDL) and / or polycaprolactone diol. In this invention, the molecular weight of the polyester diol is preferably between 1000 and 4000.
[0051] In this invention, the isocyanate monomer preferably includes one or more of isophorone diisocyanate (IPDI), toluene diisocyanate, and hexamethylene diisocyanate.
[0052] In this invention, the molar ratio of the polyester diol to the isocyanate monomer is preferably 1:1 to 5, and more preferably 1:2 to 4.
[0053] In this invention, the catalyst preferably comprises dibutyltin dilaurate. In this invention, the molar ratio of the catalyst to the isocyanate monomer is preferably 0.009 to 0.1:1.
[0054] In this invention, the solvent used to dissolve and mix the polyester glycol, isocyanate monomer, and catalyst is preferably an organic solvent, which preferably includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP). In this invention, the mass ratio of the polyester glycol to the organic solvent is preferably 1:1 to 300.
[0055] In this invention, the dissolution and mixing of the polyester glycol, isocyanate monomer, and catalyst preferably includes the following steps: dissolving the polyester glycol in an organic solvent, and then adding the isocyanate monomer and catalyst. In this invention, the dissolution temperature of the polyester glycol is preferably 20–150°C, and the dissolution time is preferably 0.5–3 hours; the dissolution of the polyester glycol is preferably carried out under an oil bath and nitrogen protection.
[0056] In this invention, the temperature of the nucleophilic addition reaction is preferably 60–90°C, more preferably 70–80°C; the time is preferably 2–6 hours. In this invention, the nucleophilic addition reaction is preferably carried out under stirring conditions.
[0057] After the nucleophilic addition reaction, the present invention proceeds with subsequent reactions without any further processing.
[0058] After obtaining the polyurethane prepolymer, the present invention dissolves and mixes the polyurethane prepolymer, aliphatic diamine and phenanthroline diphenylamine, and carries out a polymerization reaction to obtain crosslinked polyurethane.
[0059] In this invention, the aliphatic diamine preferably includes one or more of 4,4'-diaminodicyclohexylmethane (DDCM), methylcyclohexanediamine (HTDA), and ethylenediamine.
[0060] In this invention, the reagent used to dissolve and mix the polyurethane prepolymer, aliphatic diamine, and phenanthrene diphenylamine is preferably an organic solvent, and the organic solvent preferably includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP).
[0061] In this invention, the phenanthroline diphenylamine preferably comprises 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine.
[0062] In this invention, the molar ratio of the aliphatic diamine to phenanthroline diphenylamine is preferably 1:0.2 to 1. In this invention, the mass ratio of the aliphatic diamine to the organic solvent is preferably 1:1 to 300. In this invention, the mass ratio of the phenanthroline diphenylamine to the organic solvent is preferably 1:1 to 300.
[0063] In this invention, the molar ratio of the fatty diamine to the isocyanate monomer is preferably 1:1 to 5, and more preferably 1:2.5.
[0064] In this invention, the dissolution and mixing of the polyurethane prepolymer, aliphatic diamine, and phenanthroline diphenylamine preferably includes the following steps: dissolving the aliphatic diamine in an organic solvent to obtain an aliphatic diamine solution; dissolving the phenanthroline diphenylamine in an organic solvent to obtain a phenanthroline diphenylamine solution; performing a first mixing of the aliphatic diamine solution and the polyurethane prepolymer, and then adding the phenanthroline diphenylamine solution. In this invention, the temperature of the first mixing is preferably 80°C, and the time is preferably 1 hour; the first mixing is preferably carried out under stirring conditions.
[0065] In this invention, the polymerization reaction is preferably carried out at a temperature of 50–80°C and for a duration of 1–5 hours. Preferably, the polymerization reaction is conducted under stirring conditions.
[0066] After the polymerization reaction, the present invention preferably proceeds with subsequent operations directly on the resulting system without any post-processing.
[0067] After obtaining the cross-linked polyurethane, the present invention dissolves and mixes the cross-linked polyurethane and organic cuprous oxide to carry out a first coordination reaction to obtain the interlocked polyurethane material.
[0068] In this invention, the organic cuprous metal preferably comprises tetraethyl copper tetrafluoroborate. In this invention, the molar ratio of the organic cuprous metal to phenanthrene diphenylamine is preferably 0.1–1:0.2–1, more preferably 1:2.
[0069] In this invention, the reagent used to dissolve and mix the crosslinked polyurethane and the organic cuprous oxide is preferably an organic solvent, which preferably includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP). In this invention, the mass ratio of the organic cuprous oxide to the organic solvent is preferably 1:1 to 300.
[0070] In this invention, the preferred method of dissolving and mixing the cross-linked polyurethane and the organic cuprous oxide includes: dissolving the organic cuprous oxide in an organic solvent to obtain an organic cuprous oxide solution; and mixing the organic cuprous oxide solution with the cross-linked polyurethane.
[0071] In this invention, the temperature of the first coordination reaction is preferably 40-80°C, more preferably 50-70°C; and the time is preferably 3-5 hours.
[0072] In this invention, the interlocking polyurethane material is preferably a thin-film interlocking polyurethane material. When preparing the thin-film interlocking polyurethane material, this invention preferably places the liquid obtained from the first coordination reaction in a mold and dries it. In this invention, the mold is preferably made of Teflon. In this invention, the drying method is preferably vacuum drying, the vacuum drying temperature is preferably 80°C, the time is preferably 24 hours, and the vacuum drying is preferably carried out in a vacuum drying oven.
[0073] This invention also provides a method for preparing an interlocking polyurethane-polyimide material, comprising the following steps:
[0074] Crosslinked polyurethane was prepared according to the preparation method described in the above technical solution;
[0075] The cross-linked polyurethane, polyimide and organic cuprous oxide are dissolved and mixed, and a second coordination reaction is carried out to obtain the interlocked polyurethane-polyimide material.
[0076] The polyimide is obtained by sequentially acylation and imidization of 4,4'-oxybisphthalic anhydride and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine.
[0077] The present invention prepares cross-linked polyurethane according to the preparation method described in the above technical solution.
[0078] In this invention, the preparation method of the crosslinked polyurethane is preferably the same as the above-described technical solution, and will not be repeated here.
[0079] After obtaining the cross-linked polyurethane, the present invention dissolves and mixes the cross-linked polyurethane, polyimide and organic cuprous oxide, and carries out a second coordination reaction to obtain the interlocked polyurethane-polyimide material.
[0080] In this invention, the polyimide is obtained by sequentially acylation and imidization of 4,4'-oxybisphthalic anhydride and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine.
[0081] In this invention, the polyimide is preferably used in the form of a polyimide solution. Specifically, the method for preparing the polyimide solution preferably includes the following steps:
[0082] 4,4'-O-bisphthalic anhydride, 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine and an organic solvent were mixed and subjected to an acylation reaction under nitrogen atmosphere to obtain a polyamic acid solution.
[0083] The polyamic acid solution is subjected to imidization treatment to obtain the polyimide solution.
[0084] In this invention, the organic solvent preferably includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP). In this invention, the mass ratio of the 4,4'-oxophthalic anhydride to the organic solvent is preferably 1:1 to 300. In this invention, the mass ratio of the 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine to the organic solvent is preferably 1:1 to 300. In this invention, the molar ratio of the 4,4'-oxophthalic anhydride to 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine is preferably 1 to 1.2:1 to 1.2, more preferably 1:1. In this invention, the acylation reaction is preferably carried out under ice bath and nitrogen conditions, and the acylation reaction time is preferably 12 to 36 hours. In this invention, the temperature of the imidization treatment is preferably 200-280°C, more preferably 230-250°C; and the time is preferably 30 min-6 h.
[0085] In this invention, the organic cuprous oxide is preferably tetraethyl copper tetrafluoroborate. In this invention, the ratio of the total molar amount of phenanthroline diphenylamine in the crosslinked polyurethane and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine in the polyimide to the molar amount of the organic cuprous oxide is preferably 0.2–1:0.15–1, more preferably 2:1.
[0086] In this invention, the molar ratio of phenanthroline diphenylamine in the crosslinked polyurethane to 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine in the polyimide is preferably 0.1–1:0.1–1, more preferably 0.2:0.1–0.3, and specifically preferably 0.2:0.1, 0.2:0.2, or 0.2:0.3. In this invention, the reagent used to dissolve and mix the crosslinked polyurethane, polyimide, and organic cuprous oxide is preferably an organic solvent, which preferably includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP).
[0087] In this invention, the dissolution and mixing of the cross-linked polyurethane, polyimide, and organic cuprous oxide preferably includes the following steps: dissolving the organic cuprous oxide in an organic solvent to obtain an organic cuprous oxide solution; and mixing the organic cuprous oxide solution, the cross-linked polyurethane, and the polyimide.
[0088] In this invention, the temperature of the second coordination reaction is preferably 40-80°C, more preferably 50-70°C; and the time is preferably 3-5 hours.
[0089] In this invention, the interlocking polyurethane-polyimide material is preferably a thin-film interlocking polyurethane-polyimide material. When preparing the thin-film interlocking polyurethane-polyimide material, this invention preferably places the liquid obtained from the second coordination reaction in a mold for drying. In this invention, the mold is preferably made of Teflon. In this invention, the drying method is preferably vacuum drying, the vacuum drying temperature is preferably 80°C, the time is preferably 24 hours, and the vacuum drying is preferably carried out in a vacuum drying oven.
[0090] The following detailed description, in conjunction with embodiments, illustrates the preparation methods of the interlocking polyurethane material and the interlocking polyurethane-polyimide material provided by the present invention. However, these descriptions should not be construed as limiting the scope of protection of the present invention.
[0091] Example 1
[0092] (1) Weigh 2.0g and 1.00mmol of polycarbonate diol PCDL-2000 with a molecular weight of 2000g / mol and 10g of DMAc and mix them in a three-necked flask. Stir vigorously for 1h under oil bath conditions at 120℃ and nitrogen atmosphere to obtain a mixed solution of PCDL-2000 and DMAc.
[0093] (2) In the reaction apparatus, the reaction temperature was lowered to 80°C, and 0.45 g of isophorone diisocyanate (IPDI) and 0.02 g of dibutyltin dilaurate (0.02 mmol) were added. After stirring vigorously for 3 hours, polyurethane prepolymer was obtained.
[0094] (3) Mix 0.168 g and 0.80 mmol of 4,4'-diaminodicyclohexylmethane with 10 g of DMAc and add the mixture to the reaction system. Stir vigorously at 80 °C for about 1 h.
[0095] (4) After uniformly mixing 72 mg and 0.20 mmol of 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine with 5 g of DMAc, and after forming a uniform mixed solution, add it to the reaction system, and continue stirring at 80 °C for 1 h. The polymerization reaction is completed, and a polyurethane solution is obtained, in which about 2700 mg of polyurethane is obtained.
[0096] (5) After uniformly mixing 31.4 mg and 0.10 mmol of tetrafluoroborate tetraethyl copper with 3 g of DMAc, and waiting to form a uniform mixed solution, add it to the polyurethane solution to carry out a coordination reaction. The reaction temperature is 50 °C and the time is 5 h to obtain an interlocked polyurethane material.
[0097] (6) Pour the interlocking polyurethane material into a Teflon mold, place it in a vacuum drying oven at 80°C, and dry for 24 hours to obtain a solid interlocking polyurethane material, named Example 1.
[0098] Example 2
[0099] Repeat steps 1 to 4 in Example 1 to obtain an equal amount of polyurethane solution, wherein 2700 mg of polyurethane is contained.
[0100] (5) Weigh 31 mg and 0.10 mmol of 4,4'-oxophthalic anhydride and 3.1 g of NMP, mix them evenly, and add them to a three-necked flask placed in an ice bath and nitrogen atmosphere. Then weigh 36 mg and 0.10 mmol of 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine and 3.6 g of NMP, add them to the three-necked flask after they are completely dissolved, and react for 24 h to obtain a polyamic acid solution.
[0101] (6) The three-necked flask containing the polyamic acid solution was placed in an electric heating mantle at a temperature of 230°C for imidization treatment for about 2 hours to obtain a polyimide solution, which was kept for later use. The mass of the polyimide was about 67 mg.
[0102] (7) Weigh 47.1 mg and 0.15 mmol of tetrafluoroborate tetraethyl copper and 5 g of DMAc, mix them, and add the mixture into a reaction apparatus containing polyurethane solution and polyimide solution to carry out a coordination reaction. The reaction temperature is 50 °C and the time is 5 h to obtain interlocked polyurethane-polyimide material.
[0103] (8) Pour the interlocking polyurethane-polyimide material into a Teflon mold, place it in a vacuum drying oven at 80°C, and dry for 24 hours to obtain solid interlocking polyurethane-polyimide, which is named Example 2.
[0104] Example 3
[0105] Repeat steps 1 to 4 in Example 1 to obtain an equal amount of polyurethane solution, wherein approximately 2700 mg of polyurethane is contained.
[0106] (5) Weigh 62 mg and 0.20 mmol of 4,4'-oxophthalic anhydride and 6.2 g of NMP, mix them evenly, and add them to a three-necked flask placed in an ice bath and nitrogen atmosphere. Then weigh 72 mg and 0.20 mmol of 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine and 7.2 g of NMP, add them to the three-necked flask after they are completely dissolved, and react for 24 h to obtain a polyamic acid solution.
[0107] (6) The three-necked flask containing the polyamic acid solution was placed in an electric heating mantle at a temperature of 230°C for imidization treatment for 2 hours to obtain a polyimide solution, which was kept for later use. The mass of the polyimide was approximately 134 mg.
[0108] (7) Weigh out 62.8 mg of 0.20 mmol of tetrafluoroborate tetraethyl copper and 6 g of DMAc, mix them, and add the mixture into a reaction apparatus containing polyurethane solution and polyimide solution to carry out a coordination reaction. The reaction temperature is 50 °C and the time is 5 h to obtain interlocked polyurethane-polyimide material.
[0109] (8) Pour the interlocking polyurethane-polyimide material into a Teflon mold, place it in a vacuum drying oven at 80°C, and dry for 24 hours to obtain a solid interlocking polyurethane-polyimide material, named Example 3.
[0110] Example 4
[0111] Repeat steps 1 to 4 in Example 1 to obtain an equal amount of polyurethane solution, wherein approximately 2700 mg of polyurethane is contained.
[0112] (5) Weigh 93 mg and 0.30 mmol of 4,4'-oxophthalic anhydride and 9.3 g of NMP, mix them evenly, and add them to a three-necked flask placed in an ice bath and nitrogen environment. Then weigh 108 mg and 0.30 mmol of 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine and 10 g of NMP. After they are completely dissolved, add them to the three-necked flask and react for 24 h to obtain a polyamic acid solution.
[0113] (6) The three-necked flask containing the polyamic acid solution is placed in an electric heating mantle at a temperature of 230°C for imidization treatment for about 2 hours to obtain a polyimide solution, which is kept for later use. The mass of the polyimide is about 201 mg.
[0114] (7) Weigh out 78.5 mg of 0.25 mmol of tetrafluoroborate tetraethyl copper and 7 g of DMAc, mix them, and add the mixture into a reaction apparatus containing polyurethane solution and polyimide solution to carry out a coordination reaction. The reaction temperature is 50 °C and the time is 5 h to obtain interlocked polyurethane-polyimide material.
[0115] (8) Pour the interlocking polyurethane-polyimide material into a Teflon mold, place it in a vacuum drying oven at 80°C, and dry for 24 hours to obtain a solid interlocking polyurethane-polyimide material, named Example 4.
[0116] Characterization and performance analysis
[0117] 1. Infrared spectral analysis:
[0118] As is well known, Fourier transform infrared (FT-IR) spectroscopy is a powerful tool for studying the efficient synthesis of polymers. The FT-IR spectra were acquired on a Nicolet Nexus 870 spectrometer, with a scan range of 4000 to 500 cm⁻¹. -1 The results are shown Figure 1 . Figure 1 In the middle, at 2270cm -1 The absence of a stretching vibration peak corresponding to the isocyanate (-NCO) group nearby indicates that the -NCO group of the isocyanate was completely consumed. (1740 cm⁻¹) -1 The vibrational peak attributable to the carbonyl group (-C=O-) in the urethane (-NHCOO-) group, 1242 cm⁻¹ -1 The characteristic peak is the vibrational peak of the carbon-oxygen bond (-CO-) in the -NHCOO- group, confirming the presence of the urethane bond, i.e., the successful preparation of the polyurethane material. Furthermore, a peak of 1505 cm⁻¹ was observed in Examples 2-4. -1 A new peak appeared nearby, which was not observed in Example 1, at 1505 cm. -1 The stretching peak of the C=C bond in the aromatic ring of 4,4'-oxydiphthalic anhydride confirmed the successful incorporation of polyimide. In Examples 1-4, the peak at 1056 cm⁻¹... -1 Stretching vibration peaks belonging to the BF bond in the coordination compound (tetrafluoroborate tetraethyl cyanocopper) were detected at all locations, indicating the successful incorporation of metal coordination ions. This further confirms that polyurethane and polyimide have achieved "interlocking" through metal coordination bonds, namely, the successful preparation of an interlocking polyurethane material and an interlocking polyurethane-polyimide material.
[0119] 2.2 XRD Curve Analysis:
[0120] X-ray diffraction (XRD) tests were performed on a Bruker D8 Advance (BRUKER, Germany). Cu-Kα radiation, scanned from 5° to 80° at a rate of 5°min. -1 The results are shown Figure 2 . Figure 2 In the sample, only one amorphous broad peak appears at 2θ = 20°, without any obvious crystallization peak. The results indicate that the samples in the examples are all amorphous and therefore do not have a crystal structure.
[0121] 2.3 Molecular weight information:
[0122] The molecular weight was determined by gel permeation chromatography (GPC, Agilent PL-GPC50, USA) with DMF as the mobile phase. The results are shown in Table 1.
[0123] Table 1 Summary of relative molecular weight and polydispersity index for different interlocking materials
[0124]
[0125] The results in Table 1 show that the number-average molecular weight of the sample in the examples ranges from about 70,000 to 110,000, and the polydispersity index (PDI) ranges from 1.4 to 1.6, indicating that the molecular weight distribution is relatively wide.
[0126] 2.4 Mechanical Property Analysis
[0127] To evaluate the mechanical properties of the prepared polyurethane elastomer materials, the film samples prepared in Examples 1, 2, 3, and 4 were subjected to mechanical property tests (loading speed: 100 mm / min, test environment: room temperature). Stress-strain curves at a fixed tensile speed were recorded using an electronic universal tensile testing machine (Shimadzu, AG-X). All specimens were cut into dumbbell shapes (30 mm × 2 mm × 0.5 mm) to obtain reliable average values. Toughness (τ) can be defined by integrating the area under the stress-strain curve, calculated as follows (S1):
[0128]
[0129] In the formula, σ is the stress value, ε is the strain value, and εmax is the elongation at break.
[0130] The results are summarized in Table 2 and Figure 3 middle.
[0131] Table 2 Summary of elongation at break, tensile strength and toughness information for different embodiments
[0132]
[0133] From Table 2 and Figure 3 The strength, elongation, and toughness results shown indicate that the interlocking polyurethane materials and interlocking polyurethane-polyimide materials prepared by the method provided in this invention possess outstanding mechanical properties, especially their toughness, which holds a significant advantage in the polyurethane or polyimide fields. For the sample in Example 1, an interlocking polyurethane material, its mechanical strength is 52.0 MPa, and its toughness value is as high as 303.4 MJ / m. 3In the polyurethane network structure, the material exhibits the best stretchability due to the presence of weak hydrogen bonds such as urethane and urea groups, with an elongation of 1282%. For the samples in Examples 2-4, which are all interlocking polyurethane-polyimide materials, the incorporation of polyimide, which can form interlocking structures, results in more rigid structural units, leading to a significant improvement in the material's strength and modulus. Figure 3 As shown, with the gradual increase of the amount of polyimide incorporated, the modulus of the material gradually increases, while the elongation generally shows a decreasing trend. It is worth noting that for the sample of Example 3, when the optimal amount of polyimide is incorporated, the material's strength reaches a maximum of 91.4 MPa, and its toughness reaches a maximum of 448.0 MJ / m. 3 The results show that by rationally adjusting the ratio and content of polyurethane and polyimide, polymer materials with overall enhanced mechanical properties were prepared.
[0134] In summary, the interlocking polyurethane material and interlocking polyurethane-polyimide material prepared by this invention, combined with their special "interlocking" network structure, have the following enhancement mechanism related to mechanical properties.
[0135] Figure 4 This is a schematic diagram of the polyurethane-polyimide "interlocking" structure; as shown. Figure 4 As shown, the "interlocking" structure of polyurethane and polyimide is revealed. Figure 4In the diagram, PU chain represents the polyurethane segment, and PI chain represents the polyimide segment. Within the polymer network, the monovalent copper ions Cu(I) brought by tetraethyl orthocyanidate form a metal-ligand coordination interaction with 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine, namely the metal-coordinate bond Cu(I)-4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine. This non-covalent interaction connects two completely independent polymer chains, achieving a theoretical "interlocking" between the polymer chains. Unlike traditional single-polymer networks or dual-network structures, this "interlocking" structure ingeniously combines rigid polyimide chains and flexible polyurethane chains for the first time. Simultaneously, based on the interpenetrating polymer network, the incorporation of metal ions Cu(I) allows for metal coordination with phenanthroline diphenylamine in the polyurethane chain and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine in the polyimide chain, respectively. Cu(I) serves as the corresponding coordination center ion, forming metal coordination bonds. On one hand, these metal coordination bonds, as dynamically reversible supramolecular interactions, act as sacrificial bonds in the form of non-covalent bonds to dissipate energy from the external load. These sacrificial coordination bonds undergo continuous dynamic breakage and recombination during stretching, resulting in continuous energy dissipation and thus endowing the material with high elongation and excellent toughness. On the other hand, the rigid polyimide chains, with their numerous rigid benzene rings, reinforce the "interlocking" network. The rigid polyimide chains provide a robust cross-linked network structure, thereby imparting high tensile strength to the material. The flexible polyurethane chains, in turn, provide excellent toughness. The above analysis shows that, thanks to the combination of rigid and flexible polyurethane and polyimide chains, as well as the successful introduction of metal coordination bonds, the interlocking polyurethane-polyimide material prepared by this invention exhibits unique interlocking structural characteristics and outstanding mechanical properties.
[0136] 2.5 Thermal Performance Analysis
[0137] Thermogravimetric analysis (TGA) was performed on an SDT 650 simultaneous thermal analyzer (TA, USA). The test atmosphere was nitrogen, the test temperature range was room temperature to 800℃, and the heating rate was 10℃ / min. The results are shown in Table 3. Figure 5 .
[0138] Table 3 Summary of thermogravimetric temperatures in Examples 1-4
[0139]
[0140] Depend on Figure 5 As shown in Table 3, all the sample examples exhibited excellent heat resistance. The thermogravimetric temperature (T0) of the samples... dThe temperature corresponding to a 5% weight loss of the sample was within the range of 270℃ to 300℃, which is superior to most polymer materials. Around 480℃, the sample mass gradually stabilized. Due to the incorporation of the coordinating ion (tetraethyl copper tetrafluoroborate), there were residual masses in Examples 1, 2, 3, and 4, with residual masses of 4.8%, 7.3%, 9.3%, and 10.8%, respectively. Thermogravimetric analysis (TGA) results fully demonstrate that the interlocking polyurethane material and interlocking polyurethane-polyimide material prepared in this invention not only exhibit high strength, high toughness, and high stretchability, but also excellent heat resistance, showing great application potential in many high-temperature environments.
[0141] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A process for the preparation of an interlocked polyurethane material, characterized in that, Includes the following steps: A diol, isocyanate monomer, and catalyst are dissolved and mixed, and a nucleophilic addition reaction is carried out to obtain a polyurethane prepolymer; the diol includes polycarbonate diol and / or polycaprolactone diol; the molecular weight of the diol is 1000~4000; The polyurethane prepolymer, diamine, and phenanthroline diphenylamine are dissolved and mixed, and then subjected to a polymerization reaction to obtain a cross-linked polyurethane; the diamine includes one or more of 4,4'-diaminodicyclohexylmethane, methylcyclohexanediamine, and ethylenediamine. The cross-linked polyurethane and organic cuprous oxide are dissolved and mixed to carry out a first coordination reaction, thereby obtaining the interlocked polyurethane material.
2. The production method according to claim 1, characterized by, The isocyanate monomer includes one or more of isophorone diisocyanate, toluene diisocyanate and hexamethylene diisocyanate; The molar ratio of the diol to the isocyanate monomer is 1:1 to 5.
3. The preparation method according to claim 1, characterized in that, The catalyst includes dibutyltin dilaurate; The molar ratio of the catalyst to the isocyanate monomer is 0.009 to 0.1:
1.
4. The preparation method according to any one of claims 1 to 3, characterized in that, The nucleophilic addition reaction is carried out at a temperature of 60-90°C for 2-6 hours.
5. The preparation method according to claim 1, characterized in that, The phenanthroline diphenylamine includes 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine; The molar ratio of the diamine to phenanthrene-2-phenylamine is 1:0.2~1; The molar ratio of the diamine to the isocyanate monomer is 1:1 to 5.
6. The preparation method according to claim 1 or 5, characterized in that, The polymerization reaction is carried out at a temperature of 50-80°C for 2-5 hours.
7. The preparation method according to claim 1, characterized in that, The organic cuprous oxide comprises tetraethyl copper tetrafluoroborate; the molar ratio of the organic cuprous oxide to phenanthrene diphenylamine is 0.1~1:0.2~1.
8. The preparation method according to claim 1 or 7, characterized in that, The temperature of the first coordination reaction is 40~80℃ and the time is 3~5h.
9. A method for preparing an interlocking polyurethane-polyimide material, characterized in that, Includes the following steps: Crosslinked polyurethane was prepared according to the preparation method described in any one of claims 1 to 8; The cross-linked polyurethane, polyimide and organic cuprous oxide are dissolved and mixed, and a second coordination reaction is carried out to obtain the interlocked polyurethane-polyimide material. The polyimide is obtained by sequentially acylation and imidization of 4,4'-oxybisphthalic anhydride and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine.
10. The preparation method according to claim 9, characterized in that, The organic cuprous oxide is copper tetrafluoroborate tetraethyl cyano copper; The molar ratio of phenanthroline diphenylamine in the crosslinked polyurethane to 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine in the polyimide is 0.1~1:0.1~1; The ratio of the total amount of phenanthroline diphenylamine in the crosslinked polyurethane and 4,4'-(1,10-phenanthroline-2,9-diyl)diphenylamine in the polyimide to the amount of organic cuprous oxide is 0.2~1:0.15~1; The second coordination reaction is carried out at a temperature of 40-80℃ for 3-5 hours.