Low-cost anti-ablation copper-steel composite material and preparation method thereof

By adding W18Cr4V high-speed steel to molten copper and controlling atomization parameters, a low-cost, high-performance copper-steel composite material was prepared. This solved the problems of uncoordinated performance improvement and manufacturing of large-size, complex-shaped products in traditional processes, achieving significant improvement in material performance and cost reduction.

CN118048549BActive Publication Date: 2026-11-24UNIV OF SCI & TECH BEIJING
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410127751.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2026-11-24
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

In existing methods for preparing copper-iron alloys, the addition of high-carbon ferrochrome alloys, alloying elements, and carbides cannot synergistically improve mechanical properties, electrical and thermal conductivity, and ablation resistance. Furthermore, traditional processes are difficult to manufacture large-sized or complex-shaped products, resulting in low material utilization and high production costs.

Method used

Vacuum induction melting and atomization processes are used to add W18Cr4V high-speed steel to copper melt. Copper-steel composite powder is prepared by high-pressure gas or water atomization, followed by pressing, sintering and densification, and deformation processing. The superheat and atomization parameters are controlled to ensure uniform distribution and performance improvement.

Benefits of technology

A low-cost, high-strength, high-conductivity, high-thermal-conductivity, and excellent ablation-resistant copper-steel composite material has been developed, which can be used to manufacture large-size and complex-shaped products, reducing costs by more than 50%. It is suitable for electrical switches, electrode components, high-temperature molds, and electromagnetic propulsion tracks.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention provides a low-cost, ablation-resistant copper-steel composite material and its preparation method, relating to the technical field of copper alloy powder metallurgy. The preparation method is based on the high-temperature compatibility between copper and W18Cr4V high-speed steel. Copper-coated high-speed steel composite powder is prepared through a smelting-atomization powdering process, followed by pressing, molding, and sintering to densify the powder, thus preparing the copper-steel composite material. By adding W18Cr4V high-speed steel and precisely controlling key parameters such as overheating temperature and atomization pressure, this invention can synergistically improve the strength, hardness, wear resistance, and ablation resistance of the copper-steel composite material. Electrical conductivity, thermal conductivity, ablation resistance, and high-temperature stability are also significantly enhanced, facilitating large-scale industrial production and widespread application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of copper alloy powder metallurgy, and in particular to a low-cost ablation-resistant copper-steel composite material and its preparation method. Background Technology

[0002] Modern commercially available ablation-resistant copper-based composite materials mainly include refractory metal-copper composites (W-Cu, Mo-Cu, Cr-Cu, etc.) and carbide-copper composites (WC-Cu). These composite materials not only possess the high melting point, high ablation resistance, and high toughness of refractory metals (W, Mo, etc.) and their carbides, but also the electrical and thermal conductivity of copper. They maintain stable performance even under harsh environments such as high current, high temperature, high pressure, high strength, and high wear, making them important materials in many fields such as electrical contacts, electrodes, high-temperature molds, and electromagnetic propulsion.

[0003] Due to the significant differences in physical properties such as density, melting point, wettability, and coefficient of linear expansion between copper and refractory metals and carbides, it is difficult to prepare ablation-resistant copper-based composite materials using traditional casting methods. Hot pressing sintering and melt infiltration processes are generally employed. However, these methods have the following pressing problems: product size is limited, making it impossible to manufacture products such as large-size tracks for electromagnetic propulsion; material utilization is low, scrap recycling is difficult, and production costs are high; when the content of refractory metals and carbides is high, the continuity of the copper matrix is ​​insufficient, leading to a sharp decrease in the conductivity of the composite material, which seriously affects the service performance of the product.

[0004] For example, Chinese patent CN114289725A discloses a method for preparing a high-strength, high-conductivity, and high-wear-resistant powder metallurgy copper-iron alloy. This method prepares copper-iron alloy powder through vacuum melting and atomization processes, and then prepares plate, strip, and rod / wire copper-iron alloys through cold isostatic pressing, vacuum sintering, and deformation processing. Although a certain amount of high-carbon ferrochrome alloy is added, mainly to precipitate trace amounts (mass fraction less than 1%) of Fe and Cr dissolved in the copper matrix as fine (Fe,Cr)7C3 hard particles to improve the alloy's conductivity, it does not mention improving the copper matrix's resistance to ablation. Furthermore, it primarily uses pure iron particles as the reinforcing phase, and the iron particles have limited resistance to ablation and will soften significantly at high temperatures. Therefore, it is foreseeable that the copper matrix's resistance to ablation and high-temperature softening cannot be effectively improved.

[0005] Chinese patent CN113005446A discloses a method and apparatus for oscillating laser-induction composite cladding of wear-resistant and ablation-resistant copper-based coatings. This method requires coupling a high-frequency oscillating laser heat source with a high-frequency induction heating source to form a composite cladding heat source; an automatic powder feeder synchronously feeds copper-based composite powder into a molten pool formed on the substrate surface by the composite cladding heat source; the laser beam performs a regular high-frequency scanning motion within the molten pool. Clearly, this method is not suitable for the overall preparation of ablation-resistant copper-steel composite materials, and the composite components in the copper-based composite material are not only complex but also costly, and cannot be uniformly distributed within the copper matrix during the melting process. Chinese patent CN114892167A also suffers from the same technical problem.

[0006] Chinese patent CN117230344A discloses a copper alloy and its preparation method, which involves adding a high-entropy alloy nano-precipitate phase to a copper matrix. Obviously, the melting method, cold rolling, and subsequent two annealing treatments have a certain impact on the uniformity of the microstructure of the copper alloy. However, in reality, the temperature required to make the high-entropy alloy uniformly distributed in the cold-rolled microstructure is much higher than that in this technical solution, and the cost and process are longer. Summary of the Invention

[0007] The technical problem this invention aims to solve is that current copper-iron alloy preparation methods, which improve performance by adding high-carbon ferrochrome alloys, alloying elements, and carbides, suffer from uneven precipitate distribution and fail to synergistically improve mechanical properties, electrical and thermal conductivity, and ablation resistance. For example, sometimes higher electrical conductivity leads to lower mechanical properties; sometimes higher electrical and mechanical properties lead to lower thermal conductivity; and sometimes improved electrical and thermal conductivity result in lower mechanical and ablation resistance.

[0008] To solve the above-mentioned technical problems, the present invention provides the following technical solution:

[0009] A low-cost ablation-resistant copper-steel composite material, wherein the amount of W18Cr4V high-speed steel added is 10-60wt%, and the remainder is copper and unavoidable impurities.

[0010] Preferably, the complex-shaped parts made of low-cost, ablation-resistant copper-steel composite materials have a tensile strength of 263-422 MPa, a yield strength of 86-165 MPa, an elongation of 48-16%, an electrical conductivity of 45-67% IACS, and a thermal conductivity of 224-328 W·m. -1 ·k -1 The Vickers hardness is HV60-128, the softening temperature is 600-750℃, and the arc ablation rate is 35-68μg / C, based on 100 ablation cycles.

[0011] Preferably, the high-strength, high-conductivity, and high-wear-resistant copper-steel composite rods and wires have a tensile strength of 683-1450 MPa, a yield strength of 628-1377 MPa, a yield ratio of 0.92-0.95, an elongation of 5-16%, an electrical conductivity of 43-68% IACS, and a thermal conductivity of 237-330 W·m. -1 ·k -1 Its Vickers hardness is HV236-394, its softening temperature is 600-800℃, and its arc ablation rate is 37-64μg / C, based on 100 ablation cycles.

[0012] Preferably, when the thickness of the high-strength, high-conductivity, and high-wear-resistant copper-steel composite material strip is 0.5-25 mm, the tensile strength is 713-1360 MPa, the yield strength is 640-1265 MPa, the yield ratio is 0.90-0.93, the elongation is 3-15%, the electrical conductivity is 42-65% IACS, and the thermal conductivity is 225-320 W·m. -1 ·k -1 Its Vickers hardness is HV227-375, its softening temperature is 600-800℃, and its arc ablation rate is 35-62μg / C, based on 100 ablation cycles.

[0013] A method for preparing a low-cost ablation-resistant copper-steel composite material, comprising the following steps:

[0014] S1, Vacuum Induction Melting

[0015] Using cathode copper plates and W18Cr4V high-speed steel as raw materials, they are placed together in a crucible in the melting chamber and heated until completely melted to obtain copper-steel alloy melt.

[0016] S2, Atomization Powder Production

[0017] When the copper-steel alloy melt of S1 is overheated, the vacuum system is adjusted and the tundish is preheated at the same time. The copper-steel alloy melt is atomized into alloy droplets through the nozzle. After the alloy droplets are cooled, copper-steel composite powder containing W18Cr4V high-speed steel hard phase is obtained.

[0018] S3, Molding

[0019] The copper-steel composite powder of S2 is loaded into a rubber or silicone sleeve or a metal mold and pressed to obtain a copper-steel composite green blank.

[0020] S4, Sintering densification

[0021] The copper-steel composite green billet of S3 is sintered in a vacuum or hydrogen atmosphere to obtain a densified copper-steel composite sintered billet.

[0022] S5, Deformation Processing and Heat Treatment

[0023] The dense copper-steel composite sintered billets of S4 are finished and polished to obtain parts, or they are deformed by hot extrusion, hot forging, or hot rolling to obtain copper-steel composite rods, wires, plates, or strips, and then heat-treated according to different application requirements.

[0024] Preferably, heating in S1 requires a vacuum degree of 10. -1 -10 -3 Pa, the heating power increases in a gradient, and the melting temperature is 1200-1550℃.

[0025] Preferably, in step S2, the vacuum system is adjusted to be closed, and high-purity nitrogen or high-purity argon is introduced to the standard atmospheric pressure. To atomize the copper-steel alloy melt into alloy droplets through the nozzle, the alloy melt must first flow downward from the bottom guide nozzle of the tundish. Then, when it passes through the nozzle, the copper-steel alloy melt encounters the atomizing medium and is atomized into fine droplets. The alloy droplets are cooled rapidly inside the closed atomizing cylinder.

[0026] Preferably, the copper-steel composite powder in S2 has an average particle size of 5-75 μm, and the powder particles contain uniformly distributed W18Cr4V high-speed steel particles of 0.2-2 μm inside.

[0027] Preferably, the pressing pressure in S3 is 100-400MPa, the holding time is 10-300s, the high-pressure atomizing medium can be one or more of nitrogen, argon or water, and the atomizing pressure is 4-120MPa.

[0028] Preferably, copper-steel composite powder molding in S3 is used to manufacture complex-shaped parts, bar blanks, tube blanks, slab blanks, and irregular-shaped blanks.

[0029] Preferably, the vacuum degree of vacuum sintering in S4 needs to reach 10. -1 -10 -3 Pa, sintering temperature is 900-1100℃, holding time is 1.0-5.0h.

[0030] Preferably, the relative density of the S4 steel composite sintered billet is 98.5-100%, and after finishing and polishing, it can be directly used as an electrical contact or electrode component.

[0031] Preferably, the hot extrusion temperature in S5 is 500-900℃, the hot forging temperature is 500-850℃, and the hot rolling temperature is 600-950℃.

[0032] The technical principle of this invention is as follows:

[0033] A certain amount of W18Cr4V high-speed steel is added to the copper melt. Based on the high-temperature compatibility of Cu and Fe, the W18Cr4V high-speed steel melts into the copper melt to form an alloy melt. The copper-steel composite powder is prepared by high-pressure gas or water atomization. The copper-steel composite material sintered billet is obtained by pressing and sintering to achieve densification. The parts are obtained by finishing and polishing, or by deformation processing as needed to obtain copper-steel composite material rods, wires, plates and strips.

[0034] Because elements such as C, W, Cr, and V contained in W18Cr4V high-speed steel are difficult to dissolve in copper, it is difficult to introduce these elements into copper simultaneously using traditional methods. Adding W18Cr4V high-speed steel to the molten copper during smelting allows Fe and Cu to fuse together at high temperatures. Using Fe as a carrier, these difficult-to-dissolve elements such as C, W, Cr, and V can be introduced into the copper simultaneously. The fine W18Cr4V high-speed steel hard phase particles are uniformly distributed within the copper-steel composite powder particles, which is beneficial for the sintering and densification of the copper-steel composite powder. Furthermore, the formation of a permeable copper network within the powder gives the composite material excellent electrical and thermal conductivity. The high hardness and high-temperature stability of W18Cr4V high-speed steel particles can significantly improve the hardness, wear resistance, and high-temperature softening resistance of the copper-steel composite material.

[0035] The above technical solution has at least the following advantages compared with the existing technology:

[0036] The above-mentioned solution presents a low-cost ablation-resistant copper-steel composite material and its preparation method, which can solve the technical problems that traditional hot pressing sintering, melt infiltration and other processes cannot manufacture large-size and / or complex-shaped products, and cannot synergistically improve mechanical properties, electrical conductivity and thermal conductivity, ablation resistance and other properties.

[0037] This invention adjusts the viscosity of the composite melt by controlling its superheat, allowing it to flow smoothly through the nozzle into the atomization process. Improper superheat control can easily lead to nozzle blockage, preventing atomization from being completed. It can also cause segregation of high-speed steel in the copper melt, resulting in individual high-speed steel particles appearing in the atomized composite powder system as impurities, affecting sintering performance and electromechanical properties.

[0038] This invention strictly controls the atomization process parameters, especially atomization pressure and melt flow rate. If these parameters are not properly matched, the particle size and particle size composition of the prepared copper-steel composite powder will not meet the requirements of subsequent pressing and sintering densification. Defects such as edge chipping, corner chipping, and delamination will occur in the formed green blank, resulting in low sintering density and deteriorating the performance of sintered parts and subsequent deformation processing performance.

[0039] This invention further ensures product performance by controlling hot extrusion, hot rolling, hot forging, and heat treatment processes. The prepared material has a fine microstructure, and after heat treatment, it precipitates high-hardness, high-thermal-stability nanoscale carbide particles. The preparation process is short, the production cost is low, and it is easy to machine. It has great application potential in fields such as electrical switches, electrode components, high-temperature molds, and electromagnetic propulsion tracks. Compared with products processed by traditional smelting methods, the cost is reduced by more than 50%.

[0040] The copper-steel composite material prepared by this invention has low oxygen content, fine grains, and good plasticity and toughness. It possesses excellent comprehensive properties such as high strength, high electrical conductivity, high thermal conductivity, high wear resistance, and high ablation resistance. The content range of hard phase particles can be freely adjusted according to performance requirements. This invention overcomes the problems of low performance in hot pressing sintering and the fact that melt infiltration can only prepare high-content refractory metals, which are difficult to achieve with other processes.

[0041] In summary, compared with other traditional methods, the method of this invention, by adding W18Cr4V high-speed steel and precisely controlling key parameters such as overheating temperature and atomization pressure, can synergistically improve the strength, hardness, wear resistance, and ablation resistance of copper-steel composite materials; electrical conductivity, thermal conductivity, ablation resistance, and high-temperature stability are also significantly enhanced, which is conducive to large-scale industrial production and widespread use. Detailed Implementation

[0042] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the described embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0043] A low-cost ablation-resistant copper-steel composite material, wherein the amount of W18Cr4V high-speed steel added is 10-60wt%, and the remainder is copper and unavoidable impurities.

[0044] Specifically, the complex-shaped components made of low-cost, ablation-resistant copper-steel composite materials exhibit tensile strengths of 263-422 MPa, yield strengths of 86-165 MPa, elongation of 48-16%, electrical conductivity of 45-67% IACS, and thermal conductivity of 224-328 W·m. -1 ·k -1 The Vickers hardness is HV60-128, the softening temperature is 600-750℃, and the arc ablation rate is 35-68μg / C, based on 100 ablation cycles.

[0045] Specifically, the high-strength, high-conductivity, and high-wear-resistant copper-steel composite rods and wires have a tensile strength of 683-1450 MPa, a yield strength of 628-1377 MPa, a yield ratio of 0.92-0.95, an elongation of 5-16%, an electrical conductivity of 43-68% IACS, and a thermal conductivity of 237-330 W·m. -1 ·k -1 Its Vickers hardness is HV236-394, its softening temperature is 600-800℃, and its arc ablation rate is 37-64μg / C, based on 100 ablation cycles.

[0046] Specifically, when the thickness of the high-strength, high-conductivity, and high-wear-resistant copper-steel composite strip is 0.5-25 mm, the tensile strength is 713-1360 MPa, the yield strength is 640-1265 MPa, the yield ratio is 0.90-0.93, the elongation is 3-15%, the electrical conductivity is 42-65% IACS, and the thermal conductivity is 225-320 W·m. -1 ·k -1 Its Vickers hardness is HV227-375, its softening temperature is 600-800℃, and its arc ablation rate is 35-62μg / C, based on 100 ablation cycles.

[0047] A method for preparing a low-cost ablation-resistant copper-steel composite material, comprising the following steps:

[0048] S1, Vacuum Induction Melting

[0049] Using cathode copper plates and W18Cr4V high-speed steel as raw materials, they are placed together in a crucible in the melting chamber and heated until completely melted to obtain copper-steel alloy melt.

[0050] S2, Atomization Powder Production

[0051] When the copper-steel alloy melt of S1 is overheated, the vacuum system is adjusted and the tundish is preheated at the same time. The copper-steel alloy melt is atomized into alloy droplets through the nozzle. After the alloy droplets are cooled, copper-steel composite powder containing W18Cr4V high-speed steel hard phase is obtained.

[0052] S3, Molding

[0053] The copper-steel composite powder of S2 is loaded into a rubber or silicone sleeve or a metal mold and pressed to obtain a copper-steel composite green blank.

[0054] S4, Sintering densification

[0055] The copper-steel composite green billet of S3 is sintered in a vacuum or hydrogen atmosphere to obtain a densified copper-steel composite sintered billet.

[0056] S5, Deformation Processing and Heat Treatment

[0057] The dense copper-steel composite sintered billets of S4 are finished and polished to obtain parts, or they are deformed by hot extrusion, hot forging, or hot rolling to obtain copper-steel composite rods, wires, plates, or strips, and then heat-treated according to different application requirements.

[0058] Specifically, heating in S1 requires a vacuum level of 10. -1 -10 -3 Pa, the heating power increases in a gradient, and the melting temperature is 1200-1550℃.

[0059] Specifically, in S2, the vacuum system is adjusted to be closed, and high-purity nitrogen or high-purity argon is introduced to the standard atmospheric pressure. To atomize the copper-steel alloy molten liquid into alloy droplets through the nozzle, the alloy molten liquid needs to flow downward from the bottom guide nozzle of the tundish. Then, when it passes through the nozzle, the copper-steel alloy molten liquid meets the atomizing medium and is atomized into fine droplets. The alloy droplets are cooled rapidly inside the closed atomizing cylinder.

[0060] Specifically, the average particle size of the copper-steel composite powder in S2 is 5-75μm, and the powder particles contain uniformly distributed 0.2-2μm W18Cr4V high-speed steel particles.

[0061] Specifically, the pressing pressure in S3 is 100-400MPa, the holding time is 10-300s, and the high-pressure atomizing medium can be one or more of nitrogen, argon or water, with an atomization pressure of 4-120MPa.

[0062] In particular, copper-steel composite powder molding in S3 is used to manufacture complex-shaped parts, bars, tubes, plates, and irregular-shaped blanks.

[0063] Specifically, the vacuum degree of vacuum sintering in S4 needs to reach 10. -1 -10 -3 Pa, sintering temperature is 900-1100℃, holding time is 1.0-5.0h.

[0064] In particular, the relative density of S4 medium steel composite sintered billet is 98.5-100%, and after finishing and polishing, it can be directly used as electrical contacts and electrode components.

[0065] Specifically, the hot extrusion temperature in S5 is 500-900℃, the hot forging temperature is 500-850℃, and the hot rolling temperature is 600-950℃.

[0066] Example 1

[0067] A low-cost ablation-resistant copper-steel composite material, wherein the content of W18Cr4V high-speed steel in the low-cost ablation-resistant copper-steel composite material is 10wt%.

[0068] A method for preparing a low-cost ablation-resistant copper-steel composite material, comprising the following steps:

[0069] S1, Vacuum Induction Melting

[0070] Using cathode copper plates and W18Cr4V high-speed steel as raw materials, they are placed together in a crucible in the melting chamber, and when the vacuum degree reaches 10... -1 Heating begins at Pa, with the heating power increasing gradually. Charcoal is used to cover the copper liquid to prevent oxidation. The copper is melted at 1200℃ for 30 minutes until it is completely melted to obtain a copper-steel alloy melt.

[0071] S2, Atomization Powder Production

[0072] After the copper-steel alloy melt of S1 is superheated to 150°C, the vacuum system is shut off, and high-purity nitrogen is introduced to the standard atmospheric pressure. At the same time, the tundish is preheated to 850°C. The alloy melt flows downward from the bottom guide nozzle of the tundish. When it passes through the nozzle, the copper-steel alloy melt meets the high-pressure nitrogen (atomization pressure of 4MPa) and is atomized into fine droplets. The atomized droplets are rapidly cooled in the closed atomization cylinder to obtain copper-steel composite powder containing carbides or hard metallic phases. The average particle size of the powder is 75μm, and 2μm W18Cr4V high-speed steel particles are uniformly distributed inside the powder particles.

[0073] S3, Cold Isostatic Pressing

[0074] The copper-steel composite powder of S2 was loaded into a silicone sleeve with a size of 150×100×25mm and subjected to cold isostatic pressing. The pressing pressure was 100MPa and the holding time was 300s, resulting in a copper-steel composite green blank with a size of 130×86×18mm.

[0075] S4, Sintering densification

[0076] The copper-steel composite green billet of S3 was sintered in a hydrogen atmosphere at a temperature of 900℃, a heating rate of 5℃ / min, and a holding time of 5h to obtain a copper-steel composite sintered billet ingot; the relative density of the copper-steel composite sintered billet ingot was 98.5%.

[0077] S5, Deformation Processing and Heat Treatment

[0078] The copper-steel composite sintered billet of S4 was preheated at 500℃ and then hot-rolled at 600℃ to obtain a copper-steel composite material sheet with a thickness of 5mm. After removing the surface oxide scale, it was cold-rolled in multiple passes to a thickness of 0.5mm, and then annealed in hydrogen at 400℃ for 1 hour.

[0079] The low-cost ablation-resistant copper-steel composite material prepared in this embodiment, with a plate thickness of 0.5 mm, exhibits a tensile strength of 713 MPa, a yield strength of 640 MPa, a yield ratio of 0.90, an elongation of 15%, an electrical conductivity of 64.7% IACS, and a thermal conductivity of 320 W·m. -1 ·k -1 It has a Vickers hardness of HV227, a softening temperature of 600℃, and an arc ablation rate of 62μg / C (based on 100 ablation cycles). It exhibits comparable ablation resistance to Cu-20W alloys prepared by hot pressing and sintering.

[0080] Example 2

[0081] A low-cost ablation-resistant copper-steel composite material, wherein the content of W18Cr4V high-speed steel in the low-cost ablation-resistant copper-steel composite material is 30wt%.

[0082] A method for preparing a low-cost ablation-resistant copper-steel composite material, comprising the following steps:

[0083] S1, Vacuum Induction Melting

[0084] Using cathode copper plates and W18Cr4V high-speed steel as raw materials, they are placed together in a crucible in the melting chamber, and when the vacuum degree reaches 10... -1 Heating begins at Pa, with the heating power increasing gradually. Charcoal is used to cover the copper liquid to prevent oxidation. The copper is melted at 1350℃ for 45 minutes until it is completely melted to obtain a copper-steel alloy melt.

[0085] S2, Atomization Powder Production

[0086] After the copper-steel alloy melt of S1 is overheated to 200°C, the vacuum system is shut off, and high-purity nitrogen is introduced to the standard atmospheric pressure. At the same time, the tundish is preheated to 950°C. The alloy melt flows downward from the bottom guide nozzle of the tundish. When it passes through the nozzle, the copper-steel alloy melt meets the high-pressure nitrogen (atomization pressure of 120MPa) and is atomized into fine droplets. The atomized droplets are rapidly cooled in the closed atomization cylinder to obtain copper-steel composite powder containing a hard phase of carbides. The average particle size of the powder is 5μm, and 0.2μm W18Cr4V high-speed steel particles are uniformly distributed inside the powder particles.

[0087] S3, Cold Isostatic Pressing

[0088] The copper-steel composite powder of S2 was loaded into a silicone sleeve with an inner cavity size of Φ95×300mm and subjected to cold isostatic pressing. The pressing pressure was 200MPa and the holding time was 90s, resulting in a copper-steel composite green blank with a diameter of Φ78×260mm.

[0089] S4, Sintering densification

[0090] The copper-steel composite green billet of S3 was sintered in a hydrogen atmosphere at a temperature of 1000℃, a heating rate of 5℃ / min, and a holding time of 3h to obtain a copper-steel composite sintered billet ingot; the relative density of the copper-steel composite sintered billet ingot was 99%.

[0091] S5, Deformation Processing and Heat Treatment

[0092] The copper-steel composite sintered billet of S4 was preheated at 500℃ and then hot-extruded at 750℃ to obtain a copper-steel composite rod with a diameter of Φ12mm. It was then drawn to a diameter of Φ3mm and subsequently subjected to quenching and three tempering heat treatments: the quenching process was to hold at 960℃ for 2 hours and then water quench; the tempering process was to hold at 560℃ for 1 hour and then furnace cool.

[0093] The low-cost ablation-resistant copper-steel composite material prepared in this embodiment, with a wire diameter of Φ3mm, exhibits a tensile strength of 887MPa, a yield strength of 833MPa, a yield ratio of 0.94, an elongation of 9%, an electrical conductivity of 51.5% IACS, and a thermal conductivity of 282W·m. -1 ·k -1 It has a Vickers hardness of HV293, a softening temperature of 750℃, and an arc ablation rate of 46μg / C (based on 100 ablation cycles). It exhibits comparable ablation resistance to Cu-50W alloys prepared by the melt infiltration method.

[0094] Example 3

[0095] A low-cost ablation-resistant copper-steel composite material, wherein the content of W18Cr4V high-speed steel in the low-cost ablation-resistant copper-steel composite material is 60wt%.

[0096] A method for preparing a low-cost ablation-resistant copper-steel composite material, comprising the following steps:

[0097] S1, Vacuum Induction Melting

[0098] Using cathode copper plates and W18Cr4V high-speed steel as raw materials, they are placed together in a crucible in the melting chamber, and when the vacuum degree reaches 10... -1 Heating begins at Pa, with the heating power increasing gradually. Charcoal is used to cover the copper liquid to prevent oxidation. The copper is melted at 1550℃ for 45 minutes until it is completely melted to obtain a copper-steel alloy melt.

[0099] S2, Atomization Powder Production

[0100] After the copper-steel alloy melt of S1 is superheated to 150°C, the vacuum system is shut off, and high-purity nitrogen is introduced to the standard atmospheric pressure. At the same time, the tundish is preheated to 1050°C. The alloy melt flows downward from the bottom guide nozzle of the tundish. When it passes through the nozzle, the copper-steel alloy melt meets the high-pressure nitrogen (atomization pressure of 40MPa) and is atomized into fine droplets. The atomized droplets are rapidly cooled in the closed atomization cylinder to obtain copper-steel composite powder containing a hard phase of carbides. The average particle size of the powder is 30μm, and 0.8μm W18Cr4V high-speed steel particles are uniformly distributed inside the powder particles.

[0101] S3, Cold Isostatic Pressing

[0102] The copper-steel composite powder of S2 was loaded into a silicone sleeve with an inner diameter of Φ65×450mm and subjected to cold isostatic pressing. The pressing pressure was 400MPa and the holding time was 30s to obtain a copper-steel composite green blank with a diameter of Φ50×420mm.

[0103] S4, Sintering densification

[0104] The S3 copper-steel composite green billet was sintered in a vacuum sintering furnace at a vacuum degree of 10. -3 Pa, sintering temperature of 1100℃, heating rate of 5℃ / min, holding time of 1h, to obtain copper-steel composite sintered billet; the relative density of the copper-steel composite sintered billet is 99.5%;

[0105] S5, Deformation Processing and Heat Treatment

[0106] The copper-steel composite sintered billet of S4 was preheated at 500℃ and then hot-forged at 800℃ to obtain a copper-steel composite bar with a diameter of Φ15mm. Then, it was quenched and tempered three times. The quenching process was to hold at 1000℃ for 2 hours and then water quench. The tempering process was to hold at 580℃ for 1 hour and then furnace cool.

[0107] The low-cost ablation-resistant copper-steel composite rods prepared in this embodiment, with a diameter of Φ15mm, exhibit a tensile strength of 1401MPa, a yield strength of 1330MPa, a yield ratio of 0.95, an elongation of 11%, an electrical conductivity of 43.1% IACS, and a thermal conductivity of 237W·m. -1 ·k -1 It has a Vickers hardness of HV394, a softening temperature of 800℃, and an arc ablation rate of 37μg / C (based on 100 ablation cycles). It exhibits comparable ablation resistance to Cu-80W alloys prepared by the melt infiltration method.

[0108] Example 4

[0109] A low-cost ablation-resistant copper-steel composite material, wherein the content of W18Cr4V high-speed steel in the low-cost ablation-resistant copper-steel composite material is 40wt%.

[0110] A method for preparing a low-cost ablation-resistant copper-steel composite material, comprising the following steps:

[0111] S1, Vacuum Induction Melting

[0112] Using cathode copper plates and W18Cr4V high-speed steel as raw materials, they are placed together in a crucible in the melting chamber, and when the vacuum degree reaches 10... -2 Heating begins at Pa, with the heating power increasing gradually. Charcoal is used to cover the copper liquid to prevent oxidation. The copper is melted at 1500℃ for 30 minutes until it is completely melted to obtain a copper-steel alloy melt.

[0113] S2, Atomization Powder Production

[0114] After the copper-steel alloy melt of S1 is overheated to 200°C, the vacuum system is shut off, and high-purity nitrogen is introduced to the standard atmospheric pressure. At the same time, the tundish is preheated to 900°C. The alloy melt flows downward from the bottom guide nozzle of the tundish. When it passes through the nozzle, the copper-steel alloy melt encounters the mixed medium of high-pressure water (atomization pressure of 80MPa) and nitrogen (pressure of 1MPa) and is atomized into fine droplets. The atomized droplets are rapidly cooled in the closed atomization cylinder to obtain copper-steel composite powder containing a hard phase of carbides. The average particle size of the powder is 7μm, and 0.6μm W18Cr4V high-speed steel particles are uniformly distributed inside the powder particles.

[0115] S3, Cold Isostatic Pressing

[0116] The copper-steel composite powder of S2 is loaded into the pressing mold of the electrical contact parts for molding. The pressing pressure is 400MPa and the holding time is 60s to obtain the copper-steel composite material electrical contact parts blank.

[0117] S4, Sintering densification

[0118] The copper-steel composite electrical contact component green blank of S3 was sintered in a hydrogen atmosphere at a sintering temperature of 1050℃, a heating rate of 3℃ / min, and a holding time of 4h to obtain a sintered ingot of copper-steel composite electrical contact component; the relative density of the copper-steel composite sintered ingot was 100%.

[0119] S5, Post-processing

[0120] The sintered ingots of S4 copper-steel composite electrical contact components were quenched and tempered three times. The quenching process involved holding at 1000℃ for 2 hours in water, followed by tempering at 580℃ for 1 hour in a furnace. After finishing and polishing, the copper-steel composite electrical contact components were obtained.

[0121] The low-cost, ablation-resistant copper-steel composite electrical contact component prepared in this embodiment has a tensile strength of 362 MPa, a yield strength of 136 MPa, an elongation of 19%, an electrical conductivity of 51% IACS, and a thermal conductivity of 259 W·m. -1 ·k -1 It has a Vickers hardness of HV104 and a softening temperature of 700℃; the arc ablation rate is 45μg / ℃ (based on 100 ablation cycles). It exhibits comparable ablation resistance to Cu-60W alloy prepared by hot pressing and sintering.

[0122] The above-mentioned solution presents a low-cost ablation-resistant copper-steel composite material and its preparation method, which can solve the technical problems that traditional hot pressing sintering, melt infiltration and other processes cannot manufacture large-size and / or complex-shaped products, and cannot synergistically improve mechanical properties, electrical conductivity and thermal conductivity, ablation resistance and other properties.

[0123] This invention adjusts the viscosity of the composite melt by controlling its superheat, allowing it to flow smoothly through the nozzle into the atomization process. Improper superheat control can easily lead to nozzle blockage, preventing atomization from being completed. It can also cause segregation of high-speed steel in the copper melt, resulting in individual high-speed steel particles appearing in the atomized composite powder system as impurities, affecting sintering performance and electromechanical properties.

[0124] This invention strictly controls the atomization process parameters, especially atomization pressure and melt flow rate. If these parameters are not properly matched, the particle size and particle size composition of the prepared copper-steel composite powder will not meet the requirements of subsequent pressing and sintering densification. Defects such as edge chipping, corner chipping, and delamination will occur in the formed green blank, resulting in low sintering density and deteriorating the performance of sintered parts and subsequent deformation processing performance.

[0125] This invention further ensures product performance by controlling hot extrusion, hot rolling, hot forging, and heat treatment processes. The prepared material has a fine microstructure, and after heat treatment, it precipitates high-hardness, high-thermal-stability nanoscale carbide particles. The preparation process is short, the production cost is low, and it is easy to machine. It has great application potential in fields such as electrical switches, electrode components, high-temperature molds, and electromagnetic propulsion tracks. Compared with products processed by traditional smelting methods, the cost is reduced by more than 50%.

[0126] The copper-steel composite material prepared by this invention has low oxygen content, fine grains, and good plasticity and toughness. It possesses excellent comprehensive properties such as high strength, high electrical conductivity, high thermal conductivity, high wear resistance, and high ablation resistance. The content range of hard phase particles can be freely adjusted according to performance requirements. This invention overcomes the problems of low performance in hot pressing sintering and the fact that melt infiltration can only prepare high-content refractory metals, which are difficult to achieve with other processes.

[0127] In summary, compared with other traditional methods, the method of this invention, by adding W18Cr4V high-speed steel and precisely controlling key parameters such as overheating temperature and atomization pressure, can synergistically improve the strength, hardness, wear resistance, and ablation resistance of copper-steel composite materials; electrical conductivity, thermal conductivity, ablation resistance, and high-temperature stability are also significantly enhanced, which is conducive to large-scale industrial production and widespread use.

[0128] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A low-cost, ablation-resistant copper-steel composite material, characterized in that, In the aforementioned low-cost ablation-resistant copper-steel composite material, the amount of W18Cr4V high-speed steel added is 10-60wt%, with the remainder being copper and unavoidable impurities; The preparation method of the low-cost ablation-resistant copper-steel composite material is as follows: S1, Vacuum Induction Melting Using cathode copper plates and W18Cr4V high-speed steel as raw materials, they are placed together in a crucible in the melting chamber and heated until completely melted to obtain copper-steel alloy melt. S2, Atomization Powder Production After the copper-steel alloy melt of S1 is overheated, the vacuum system is adjusted and the tundish is preheated. The copper-steel alloy melt is atomized into alloy droplets through the nozzle. After the alloy droplets are cooled, copper-steel composite powder containing the hard phase of W18Cr4V high-speed steel is obtained. The average particle size of the copper-steel composite powder is 5-75μm, and the powder particles contain W18Cr4V high-speed steel particles of 0.2-2 μm evenly distributed inside. S3, Molding The copper-steel composite powder of S2 is loaded into a rubber or silicone sleeve or a metal mold and pressed to obtain a copper-steel composite green blank. S4, Sintering densification The copper-steel composite green billet of S3 is sintered in a vacuum or hydrogen atmosphere to obtain a densified copper-steel composite sintered billet. S5, Deformation Processing and Heat Treatment The dense copper-steel composite sintered billets of S4 are finished and polished to obtain parts, or they are deformed by hot extrusion, hot forging, or hot rolling to obtain copper-steel composite rods, wires, plates, or strips, and then heat-treated according to different application requirements.

2. The low-cost ablation-resistant copper-steel composite material according to claim 1, characterized in that, The complex-shaped components made of low-cost, ablation-resistant copper-steel composite materials have a tensile strength of 263-422 MPa, a yield strength of 86-165 MPa, an elongation of 48-16%, an electrical conductivity of 45-67% IACS, and a thermal conductivity of 224-328 W·m. -1 ·k -1 The Vickers hardness is HV60-128, the softening temperature is 600-750℃, and the arc ablation rate is 35-68μg / C, based on 100 ablation cycles.

3. The low-cost ablation-resistant copper-steel composite material according to claim 1, characterized in that, The high-strength, high-conductivity, and high-wear-resistant copper-steel composite rods and wires have a tensile strength of 683-1450 MPa, a yield strength of 628-1377 MPa, a yield ratio of 0.92-0.95, an elongation of 5-16%, an electrical conductivity of 43-68% IACS, and a thermal conductivity of 237-330 W·m. -1 ·k -1 Its Vickers hardness is HV236-394, its softening temperature is 600-800℃, and its arc ablation rate is 37-64μg / C, based on 100 ablation cycles.

4. The low-cost ablation-resistant copper-steel composite material according to claim 1, characterized in that, When the thickness of the high-strength, high-conductivity, and high-wear-resistant copper-steel composite sheet / strip is 0.5-25 mm, the tensile strength is 713-1360 MPa, the yield strength is 640-1265 MPa, the yield-to-tensile ratio is 0.90-0.93, the elongation is 3-15%, the electrical conductivity is 42-65% IACS, and the thermal conductivity is 225-320 W·m. -1 ·k -1 Its Vickers hardness is HV227-375, its softening temperature is 600-800℃, and its arc ablation rate is 35-62μg / C, based on 100 ablation cycles.

5. A method for preparing a low-cost ablation-resistant copper-steel composite material according to any one of claims 1-4, characterized in that, The preparation method includes the following steps: S1, Vacuum Induction Melting Using cathode copper plates and W18Cr4V high-speed steel as raw materials, they are placed together in a crucible in the melting chamber and heated until completely melted to obtain copper-steel alloy melt. S2, Atomization Powder Production When the copper-steel alloy melt of S1 is overheated, the vacuum system is adjusted and the tundish is preheated at the same time. The copper-steel alloy melt is atomized into alloy droplets through the nozzle. After the alloy droplets are cooled, copper-steel composite powder containing W18Cr4V high-speed steel hard phase is obtained. S3, Molding The copper-steel composite powder of S2 is loaded into a rubber or silicone sleeve or a metal mold and pressed to obtain a copper-steel composite green blank. S4, Sintering densification The copper-steel composite green billet of S3 is sintered in a vacuum or hydrogen atmosphere to obtain a densified copper-steel composite sintered billet. S5, Deformation Processing and Heat Treatment The dense copper-steel composite sintered billets of S4 are finished and polished to obtain parts, or they are deformed by hot extrusion, hot forging, or hot rolling to obtain copper-steel composite rods, wires, plates, or strips, and then heat-treated according to different application requirements.

6. The method for preparing the low-cost ablation-resistant copper-steel composite material according to claim 5, characterized in that, Heating in S1 requires a vacuum level of 10. -1 -10 -3 Pa, the heating power increases in a gradient, and the melting temperature is 1200-1550℃.

7. The method for preparing the low-cost ablation-resistant copper-steel composite material according to claim 5, characterized in that, In S2, the vacuum system is adjusted to be closed, and high-purity nitrogen or high-purity argon is introduced to the standard atmospheric pressure. To atomize the copper-steel alloy molten liquid into alloy droplets through the nozzle, the alloy molten liquid must first flow downward from the bottom guide nozzle of the tundish. Then, when it passes through the nozzle, the copper-steel alloy molten liquid meets the atomizing medium and is atomized into fine droplets. The alloy droplets are cooled rapidly inside the closed atomizing cylinder.

8. The method for preparing the low-cost ablation-resistant copper-steel composite material according to claim 5, characterized in that, The pressing pressure in S3 is 100-400MPa, the holding time is 10-300s, and the high-pressure atomizing medium can be one or more of nitrogen, argon or water, with an atomization pressure of 4-120MPa.

9. The method for preparing the low-cost ablation-resistant copper-steel composite material according to claim 5, characterized in that, The vacuum degree in vacuum sintering in S4 needs to reach 10. -1 -10 -3 Pa, sintering temperature is 900-1100℃, holding time is 1.0-5.0h.

10. The method for preparing the low-cost ablation-resistant copper-steel composite material according to claim 5, characterized in that, The hot extrusion temperature of S5 is 500-900℃, the hot forging temperature is 500-850℃, and the hot rolling temperature is 600-950℃.

Citation Information

Patent Citations

  • Method and device for oscillating laser-induction composite cladding of wear-resistant and ablation-resistant copper-based coating

    CN113005446A

  • Preparation method of high-strength, high-conductivity and high-wear-resistance powder metallurgy copper-iron alloy

    CN114289725A

  • Copper alloy high-conductivity wear-resistant ablation-resistant coating and preparation method thereof

    CN114892167A

  • Copper alloy and preparation method thereof

    CN117230344A

  • Copper-based powder metallurgy antifriction material and preparation method thereof

    CN104384504A