Octahedral morphology copper-iron oxide material, and preparation method and application thereof
By synergistically regulating the use of sodium gluconate chelating agent and surfactant, octahedral CuFeO₂ materials were prepared via hydrothermal reaction. This solved the problems of monotonous morphology and poor performance of existing copper-iron-oxygen materials, achieving high efficiency in photoelectrocatalysis and high crystallinity, making it suitable for the field of photoelectrocatalysis.
Patent Information
- Application Number
- CN202410227434.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-29
AI Technical Summary
Existing copper-iron-oxygen materials have a single morphology and low crystallinity and purity, resulting in poor photoelectrocatalytic performance. Furthermore, the preparation methods are energy-intensive, making it difficult to achieve efficient photoelectrochemical conversion.
Using sodium gluconate as a chelating agent, combined with surfactants and alkaline solutions, octahedral CuFeO₂ materials were prepared via hydrothermal reaction. By controlling the reaction conditions and parameters, high-purity, highly crystalline copper-iron-oxygen particles were obtained.
The prepared octahedral copper-iron-oxygen material exhibits strong light absorption in the visible light region, high photocurrent density, and excellent photoelectrocatalytic performance. The operation is simple and highly reproducible.
Smart Images

Figure CN118062903B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photoelectrocatalytic materials technology, specifically relating to an octahedral copper-iron-oxygen material, its preparation method, and its application. Background Technology
[0002] With the increasing global energy consumption, fossil fuels such as oil, coal, and natural gas can no longer meet the long-term needs of human development. Therefore, it is imperative to accelerate the development and utilization of renewable, pollution-free, and green new energy sources. Solar energy is currently the largest source of renewable energy; however, there is no technology to directly store and utilize solar energy. Instead, it can be converted into other storable energy sources, primarily hydrogen storage. Photoelectrocatalysis is a technology that can directly convert solar energy into hydrogen energy and store it. CuFeO2 is a p-type semiconductor that can be used as an electrode material in photoelectrocatalysis due to its low cost and abundant resources. It is also a broadband absorber with an absorption edge covering the ultraviolet to infrared region, making it a promising photoelectric conversion absorber material that has attracted considerable attention among copper-based oxides. Methods for preparing CuFeO2 include the sol-gel method, solid-state method, and hydrothermal method. The sol-gel method is often used to prepare copper-ferrooxy thin film materials, but the resulting products have poor crystallinity, many impurities, and are often accompanied by byproducts such as CuO, Fe2O3, Cu2O, and CuFe2O4. The solid-state method typically requires sintering temperatures above 500℃, is energy-intensive, and produces products with low crystallinity and many impurities, making accurate physicochemical characterization and research impossible. The hydrothermal method offers mild preparation conditions, easily controllable process parameters, and good crystallinity, but most synthesized products have hexagonal flake or cubic block morphologies, exhibiting a lack of morphological diversity and innovative synthesis methods. Furthermore, most copper-ferrooxy photocathode materials used in photoelectrocatalysis exhibit poor photoelectrocatalytic performance and low current density. Summary of the Invention
[0003] To solve all or part of the above-mentioned technical problems, the present invention provides the following technical solutions: One objective of this invention is to provide an octahedral copper-ferrooxide material with the chemical formula CuFeO2. The material consists of octahedral particles with a copper-iron ore crystal structure, orthorhombic 3R (…). The configuration has the following unit cell parameters: a = 3.0351 Å, b = 3.0351 Å, c = 17.166 Å.
[0004] In some embodiments, the particle size of the copper ferrite material is 2~5 μm.
[0005] In some embodiments, the purity of the copper ferrite material is greater than or equal to 95%.
[0006] In some embodiments, the crystallinity of the copper ferrite material is greater than or equal to 60%.
[0007] A second objective of this invention is to provide a method for preparing an octahedral copper ferrite material, comprising: subjecting a mixed reaction system containing a divalent copper source, a trivalent iron source, a surfactant, a chelating agent, a reducing agent, and an alkali to a hydrothermal reaction at 140-200°C to obtain an octahedral copper ferrite material, wherein the chelating agent includes sodium gluconate, and the reducing agent includes n-propionaldehyde.
[0008] The copper ferrooxide material prepared by the method described above, using sodium gluconate as a chelating agent, exhibits an octahedral morphology and high purity and crystallinity. It has a band gap of 1.28 eV and strong light absorption in the 400-800 nm visible light region. With the addition of the sacrificial agent H₂O₂, the band gap is 0.6 eV. RHE The corresponding photocurrent density is 3.6 mA cm⁻¹. -2 The value is greater than that in most copper-iron-oxygen literature, demonstrating excellent photoelectrocatalytic performance.
[0009] In some embodiments, the preparation method specifically includes: A copper source, a ferric source, and a surfactant are uniformly dispersed in a solvent, and then a chelating agent containing sodium gluconate solution is added to obtain a precursor solution. The precursor solution is uniformly mixed with alkali to obtain a suspension; The suspension and the reducing agent are uniformly mixed to obtain a mixed reaction system, and then the hydrothermal reaction is carried out.
[0010] The applicant discovered that adding sodium gluconate in solution form to the mixed reaction system resulted in the formation of particles with a more pronounced octahedral morphology.
[0011] In some embodiments, the concentration of the sodium gluconate solution is 2.5 ~ 10 mmol / L.
[0012] In some embodiments, the amount of sodium gluconate solution added is such that the molar ratio of sodium gluconate, copper, and iron in the mixed reaction system is in the range of 2.5 × 10⁻⁶. -3 :1:1~1×10 -2 The ratio is 1:1. If the amount of sodium gluconate added is too low or too high, it will affect the formation of the octahedral morphology, leading to a decrease in crystallinity and thus affecting the photoelectrocatalytic performance.
[0013] In some embodiments, the preparation method specifically includes: adding an alkaline solution with an alkaline concentration of 0.125~0.5 g / mL to the precursor solution in batches at a rate of 1.5~3 mL / min while maintaining stirring to obtain the suspension. Adding a high concentration of alkali to the precursor solution will generate a large amount of heat, which will affect the formation and growth of crystal nuclei. Therefore, it needs to be added in batches (e.g., dropwise). After obtaining the suspension, it needs to be stirred until homogeneous before adding the reducing agent to the system.
[0014] In some embodiments, the volume ratio of propionaldehyde to the total amount of divalent copper source and trivalent iron source in the mixed reaction system is 20:1 to 50:1.
[0015] In some embodiments, the molar ratio of copper, iron, and surfactant in the mixed reaction system is 1:1:1 to 1:1:4.
[0016] In some embodiments, the divalent copper source includes one or a combination of copper nitrate, copper sulfate, and copper chloride.
[0017] In some embodiments, the trivalent iron source includes one or more combinations of ferric nitrate and ferric chloride.
[0018] In some embodiments, the surfactant includes one or more combinations of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium oleate, and sodium laurate. The addition of the surfactant can better disperse the particles, prevent agglomeration, and promote crystallization.
[0019] In some embodiments, the alkali includes one or a combination of sodium hydroxide and potassium hydroxide.
[0020] In some embodiments, the hydrothermal reaction uses a mixed solvent, comprising water and ethanol in a volume ratio of 1:4 to 1:12. The advantage of using a mixed solvent of water and ethanol as the hydrothermal reaction solvent is that it increases the solubility of the suspension, which is beneficial for crystal nucleus growth.
[0021] In some embodiments, the hydrothermal reaction takes 20 to 48 hours.
[0022] In some embodiments, after the hydrothermal reaction is completed, the copper-ferrooxy material obtained from the reaction is post-treated. The post-treatment includes washing the copper-ferrooxy material with one or more of water, nitric acid, and ethanol, and then removing the water. For example, the reaction product is centrifuged and washed three times with deionized water, 10% dilute nitric acid, and anhydrous ethanol, respectively, and then dried at 60–100°C for 12–18 h.
[0023] The third objective of this invention is to provide a copper ferrite material with an octahedral morphology obtained by the preparation method provided by any of the above-mentioned technical solutions.
[0024] The fourth objective of this invention is to provide the application of the octahedral copper-iron-oxygen material in any of the above-mentioned technical solutions in photoelectrocatalysis.
[0025] The fifth objective of this invention is to provide a photocathode comprising the octahedral copper-ferrooxide material described in any of the above-mentioned technical solutions.
[0026] The photoelectrocatalytic performance of the photocathode was tested using a three-electrode system in an electrolyte at pH 6.5 (electrolyte composition: 0.2 mol / L K₂HPO₄ + 0.2 mol / L KH₂PO₄ + 1.2% H₂O₂) and under monochromatic LED light (wavelength 455 nm, light intensity 63 mW cm⁻¹). -2 (Use as a light source, apply 0.5-1V) RHE Under the bias voltage condition, the photocurrent density is 0.5~5 mA cm⁻¹. -2 .
[0027] Compared with the prior art, the present invention has at least the following beneficial effects: (1) The preparation method provided by the present invention is the first to use sodium gluconate as a chelating agent to prepare copper iron oxygen particles with octahedral morphology, which have high purity and high crystallinity, and exhibit good photoelectrocatalytic performance. (2) Furthermore, the present invention adds a surfactant to regulate the water-to-alcohol ratio and the amount of alkali in the reaction system, and works with sodium gluconate to regulate the octahedral morphology of copper iron oxide, thereby obtaining copper iron oxide particles with excellent photocatalytic performance. (3) The preparation method provided by the present invention is simple to operate, highly reproducible, has a high yield, and the reaction conditions are mild. Attached Figure Description
[0028] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0029] Figure 1 These are the XRD patterns of the copper ferrite materials prepared in Examples 1-4 and Comparative Example 1 of this invention; Figure 2 Here is a SEM image of the copper-ferrooxide material prepared in Example 1; Figure 3Here is a SEM image of the copper ferrite material prepared in Example 2; Figure 4 Here is a SEM image of the copper ferrite material prepared in Example 3; Figure 5 Here is a SEM image of the copper ferrite material prepared in Example 4; Figure 6 Here is a SEM image of the copper ferrooxide material prepared in Example 1; Figure 7 This is a comparison chart of the I-V curves of the photocathodes prepared using the corresponding copper-ferrooxide materials in Example 3 and Comparative Example 1. Detailed Implementation
[0030] The technical solutions of the present invention will be described in detail below with reference to specific embodiments, so that those skilled in the art can better understand and implement the technical solutions of the present invention. The specific functional details disclosed herein should not be construed as limiting, but are merely intended to form the basis of the claims and to teach those skilled in the art to employ the representative basis of the invention in different ways in any suitable detailed embodiment.
[0031] Unless otherwise specified, all raw materials and reagents used in the specific embodiments of this invention are commercially available. Example 1
[0032] This embodiment provides an octahedral copper ferrite particle and its preparation method: 2.416 g (0.01 mol) copper sulfate trihydrate, 4.04 g (0.01 mol) ferric nitrate nonahydrate, and 2.8838 g (0.01 mol) sodium dodecyl sulfate were dissolved in 7.5 ml of deionized water and 30 ml of anhydrous ethanol and stirred until completely dissolved. Then, 10 mL of sodium gluconate solution with a concentration of 2.5 mmol / L was added and mixed evenly to obtain the precursor solution. Accurately weigh 8 g of sodium hydroxide and dissolve it in 35 mL of deionized water. Then add the sodium hydroxide solution dropwise to the above precursor solution. After stirring for 30 minutes, add 1 mL of n-propanal and continue stirring for 30 minutes to obtain a mixed reaction system. The mixed reaction system was then transferred to a reaction vessel and placed in an electronic drying oven, where it was reacted at 180°C for 36 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The supernatant was discarded, and the sample was washed three times with distilled water, 10% dilute nitric acid, and anhydrous ethanol. Finally, the sample was placed in a constant temperature drying oven and dried at 80°C for 12 h to obtain octahedral copper-iron-oxygen particles. Example 2
[0033] 2.416 g (0.01 mol) copper sulfate trihydrate, 4.04 g (0.01 mol) ferric nitrate nonahydrate, and 2.8838 g (0.01 mol) sodium dodecyl sulfate were dissolved in 7.5 ml of deionized water and 30 ml of anhydrous ethanol and stirred until completely dissolved. Then, 10 mL of 5 mmol / L sodium gluconate solution was added and mixed thoroughly to obtain the precursor solution. Accurately weigh 8 g of sodium hydroxide and dissolve it in 35 mL of deionized water. Then add the sodium hydroxide solution dropwise to the above precursor solution. After stirring for 30 minutes, add 1 mL of n-propanal and continue stirring for 30 minutes to obtain a mixed reaction system. The mixed reaction system was then transferred to a reaction vessel and placed in an electronic drying oven, where it was reacted at 180°C for 36 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The supernatant was discarded, and the sample was washed three times with distilled water, 10% dilute nitric acid, and anhydrous ethanol. Finally, the sample was placed in a constant temperature drying oven and dried at 80°C for 12 h to obtain octahedral copper-iron oxide particles. Example 3
[0034] 2.416 g (0.01 mol) copper sulfate trihydrate, 4.04 g (0.01 mol) ferric nitrate nonahydrate, and 2.8838 g (0.01 mol) sodium dodecyl sulfate were dissolved in 7.5 ml of deionized water and 30 ml of anhydrous ethanol and stirred until completely dissolved. Then, 10 mL of 7 mmol / L sodium gluconate solution was added and mixed thoroughly to obtain the precursor solution. Accurately weigh 8 g of sodium hydroxide and dissolve it in 35 mL of deionized water. Then add the sodium hydroxide solution dropwise to the above precursor solution. After stirring for 30 minutes, add 1 mL of n-propanal and continue stirring for 30 minutes to obtain a mixed reaction system. The mixed reaction system was then transferred to a reaction vessel and placed in an electronic drying oven, where it was reacted at 180°C for 36 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The supernatant was discarded, and the sample was washed three times with distilled water, 10% dilute nitric acid, and anhydrous ethanol. Finally, the sample was placed in a constant temperature drying oven and dried at 80°C for 12 h to obtain octahedral copper-iron-oxygen particles.
[0035] The octahedral copper ferrite particles prepared in this embodiment were used to fabricate a photocathode. The fabrication method is the same as that mentioned in DOI: 10.1039 / c2sc21845c.
[0036] The iv curve of the photocathode prepared in this embodiment is as follows: Figure 7 As shown.
[0037] Using the aforementioned photocathode, platinum wire as the counter electrode, and Ag / AgCl as the reference electrode, a three-electrode system was constructed. The photoelectrocatalytic performance of the photocathode was tested in an electrolyte solution of 0.2 M K₂HPO₄ + 0.2 M KH₂PO₄ + 1.2% H₂O₂ at pH 6.5, using monochromatic LED light (wavelength 455 nm, light intensity 63 mW cm⁻¹). -2 ( ) is used as the light source, and a voltage of 0.5–1V is applied to the electrodes. RHE After biasing, the photocurrent density is 0.5–5 mA cm⁻¹. -2 . Example 4
[0038] 2.416 g (0.01 mol) copper sulfate trihydrate, 4.04 g (0.01 mol) ferric nitrate nonahydrate, and 2.8838 g (0.01 mol) sodium dodecyl sulfate were dissolved in 7.5 ml of deionized water and 30 ml of anhydrous ethanol and stirred until completely dissolved. Then, 10 mL of 10 mmol / L sodium gluconate solution was added and mixed thoroughly to obtain the precursor solution. Accurately weigh 8 g of sodium hydroxide and dissolve it in 35 mL of deionized water. Then add the sodium hydroxide solution dropwise to the above precursor solution. After stirring for 30 minutes, add 1 mL of n-propanal and continue stirring for 30 minutes to obtain a mixed reaction system. The mixed reaction system was then transferred to a reaction vessel and placed in an electronic drying oven, where it was reacted at 180°C for 36 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The supernatant was discarded, and the sample was washed three times with distilled water, 10% dilute nitric acid, and anhydrous ethanol. Finally, the sample was placed in a constant temperature drying oven and dried at 80°C for 12 h to obtain octahedral copper-iron oxide particles. Example 5
[0039] 4.832 g (0.02 mol) copper sulfate trihydrate, 8.08 g (0.02 mol) ferric nitrate nonahydrate, and 6.9695 g (0.02 mol) sodium dodecylbenzenesulfonate were dissolved in 15 ml of deionized water and 60 ml of anhydrous ethanol and stirred until completely dissolved. Then, 10 mL of 10 mmol / L sodium gluconate solution was added and mixed thoroughly to obtain the precursor solution. Accurately weigh 16 g of sodium hydroxide and dissolve it in 70 mL of deionized water. Then, add the sodium hydroxide solution dropwise to the above precursor solution and stir for 30 minutes. Add 2 mL of n-propanal and continue stirring for 30 minutes to obtain a mixed reaction system. The mixed reaction system was then transferred to a reaction vessel and placed in an electronic drying oven, where it was reacted at 180°C for 36 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The supernatant was discarded, and the sample was washed three times with distilled water, 10% dilute nitric acid, and anhydrous ethanol. Finally, the sample was placed in a constant temperature drying oven and dried at 80°C for 12 h to obtain octahedral copper-iron oxide particles. Example 6
[0040] 4.832 g (0.02 mol) copper sulfate trihydrate, 8.08 g (0.02 mol) ferric nitrate nonahydrate, and 5.7676 g (0.02 mol) sodium dodecyl sulfate were dissolved in 15 ml of deionized water and 30 ml of anhydrous ethanol and stirred until completely dissolved. Then, 10 mL of 10 mmol / L sodium gluconate solution was added and mixed thoroughly to obtain the precursor solution. Accurately weigh 10 g of sodium hydroxide and dissolve it in 35 mL of deionized water. Then add the sodium hydroxide solution dropwise to the above precursor solution. After stirring for 30 minutes, add 1 mL of n-propanal and continue stirring for 30 minutes to obtain a mixed reaction system. The mixed reaction system was then transferred to a reaction vessel and placed in an electronic drying oven, where it was reacted at 180°C for 36 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The supernatant was discarded, and the sample was washed three times with distilled water, 10% dilute nitric acid, and anhydrous ethanol. Finally, the sample was placed in a constant temperature drying oven and dried at 80°C for 12 h to obtain octahedral copper-iron-oxygen particles. Example 7
[0041] 2.416 g (0.01 mol) copper sulfate trihydrate, 4.04 g (0.01 mol) ferric nitrate nonahydrate, and 11.5352 g (0.04 mol) sodium dodecyl sulfate were dissolved in 3 ml of deionized water and 36 ml of anhydrous ethanol and stirred until completely dissolved. Then, 10 mL of sodium gluconate solution with a concentration of 2.5 mmol / L was added and mixed evenly to obtain the precursor solution. Accurately weigh 4.375 g of sodium hydroxide and dissolve it in 35 mL of deionized water. Then, add the sodium hydroxide solution dropwise to the above precursor solution and stir for 30 minutes. Add 0.4 mL of n-propanal and continue stirring for 30 minutes to obtain a mixed reaction system. The mixed reaction system was then transferred to a reaction vessel and placed in an electronic drying oven, where it was reacted at 140°C for 20 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The supernatant was discarded, and the sample was washed three times with distilled water, 10% dilute nitric acid, and anhydrous ethanol. Finally, the sample was placed in a constant temperature drying oven and dried at 80°C for 12 h to obtain octahedral copper-iron-oxygen particles. Example 8
[0042] 2.416 g (0.01 mol) copper sulfate trihydrate, 4.04 g (0.01 mol) ferric nitrate nonahydrate, and 5.7676 g (0.02 mol) sodium dodecylbenzenesulfonate were dissolved in 5 ml of deionized water and 40 ml of anhydrous ethanol and stirred until completely dissolved. Then, 10 mL of sodium gluconate solution with a concentration of 2.5 mmol / L was added and mixed evenly to obtain the precursor solution. Accurately weigh 17.5g of sodium hydroxide, dissolve it in 35 mL of deionized water, then add the sodium hydroxide solution dropwise to the above precursor solution, stir for 30 minutes, add 0.6 mL of n-propanal, and continue stirring for 30 minutes to obtain a mixed reaction system; The mixed reaction system was then transferred to a reaction vessel and placed in an electronic drying oven, where it was reacted at 200°C for 48 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The supernatant was discarded, and the sample was washed three times with distilled water, 10% dilute nitric acid, and anhydrous ethanol. Finally, the sample was placed in a constant temperature drying oven and dried at 80°C for 12 h to obtain octahedral copper-iron-oxygen particles.
[0043] Compare with Example 1
[0044] 4.832 g (0.02 mol) copper sulfate trihydrate, 8.08 g (0.02 mol) ferric nitrate nonahydrate, and 5.7676 g (0.02 mol) sodium dodecyl sulfate were dissolved in 15 ml of deionized water and 60 ml of anhydrous ethanol and stirred until completely dissolved to obtain the precursor solution. Accurately weigh 16 g of sodium hydroxide and dissolve it in 70 mL of deionized water. Then, add the sodium hydroxide solution dropwise to the above precursor solution and stir for 30 minutes. Add 2 mL of n-propanal and continue stirring for 30 minutes to obtain a mixed reaction system. The mixed reaction system was then transferred to a reaction vessel and placed in an electronic drying oven, where it was reacted at 180°C for 36 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The supernatant was discarded, and the sample was washed three times with distilled water, 10% dilute nitric acid, and anhydrous ethanol. Finally, the sample was placed in a constant temperature drying oven and dried at 80°C for 12 h to obtain hexagonal plate-shaped copper ferrite particles.
[0045] The hexagonal copper ferrite particles prepared in Example 1 were used to fabricate a photocathode material. The preparation method was the same as in Example 3, and its I-V curve is shown below. Figure 7As shown. The test environment was the same as in Example 3, namely, the photoelectrocatalytic performance was tested in an electrolyte of 0.2 M K₂HPO₄ + 0.2 MKH₂PO₄ + 1.2% H₂O₂ at pH 6.5, using a three-electrode system and LED monochromatic light (wavelength 455 nm, light intensity 63 mW cm⁻¹). -2 ( ) is the light source.
[0046] Figure 1 The XRD patterns of the copper ferrite materials prepared in Examples 1-4 and Comparative Example 1 of the present invention are shown. Figure 2 , Figure 3 , Figure 4 , Figure 5 These are SEM images of the copper ferrite materials prepared in Examples 1, 2, 3, and 4, respectively. Figure 6 This is a SEM image of the copper-ferrooxide material prepared in Example 1. (Comparison) Figures 2-5 , Figure 6 It can be seen that the copper ferrite particles prepared by the method provided by the present invention exhibit a typical octahedral morphology with a particle size of about 2~5μm, while the copper ferrite material prepared by Comparative Example 1 has a hexagonal plate-like structure.
[0047] Compare with Example 2
[0048] The only difference from Example 1 is that the concentration of the sodium gluconate solution was 0.1 mmol / L, the amount added was 10 mL, and the morphology of the prepared copper-iron oxide was hexagonal plate-like with a band gap of around 1.36 eV. The light absorption capacity was weaker compared to the octahedral morphology, and the photoelectrocatalytic performance was 0.6 V with the addition of the sacrificial agent H₂O₂. RHE The corresponding photocurrent density is 1.2 mA cm⁻¹. -2 .
[0049] Compare with Example 3
[0050] The only difference from Example 1 is that the concentration of the sodium gluconate solution was 20 mmol / L, the amount added was 10 mL, the morphology of the prepared copper-iron oxide was hexagonal plate-like, the band gap of the material was around 1.4 eV, the light absorption capacity was weaker compared to the octahedral morphology, and the photoelectrocatalytic performance was 0.6 V with the addition of the sacrificial agent H2O2. RHE The corresponding photocurrent density is 2 mA cm⁻¹ -2 .
[0051] Compare with Example 4
[0052] The only difference from Example 1 is that the hydrothermal reaction temperature is 120°C; otherwise, the process is the same as in Example 1. The resulting copper-ferrooxide material has a broken, blocky structure and contains many impurity phases, such as Fe2O. 3, Reduce the photocurrent density of the material.
[0053] Compare with Example 5
[0054] The only difference from Example 1 is that the hydrothermal reaction temperature is 220°C. The rest is the same as Example 1. The copper ferrite material prepared has an octahedral morphology, but the surface has many pores due to strong alkali corrosion, resulting in incomplete crystallization and a low photocurrent density.
[0055] All aspects, embodiments, features, and examples of this invention are to be regarded as illustrative in all respects and are not intended to limit the invention, the scope of which is defined only by the claims. Other embodiments, modifications, and uses will become apparent to those skilled in the art without departing from the spirit and scope of the invention as claimed.
[0056] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.
[0057] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims. Moreover, unless specifically stated otherwise, any use of the terms first, second, etc., does not indicate any order or importance, but is used to distinguish one element from another.
Claims
1. A method for preparing an octahedral copper ferrite material, characterized in that, include: A mixed reaction system containing a divalent copper source, a trivalent iron source, a surfactant, a chelating agent, a reducing agent, and a base is subjected to a hydrothermal reaction at 140–200 °C to obtain an octahedral copper-ferrooxide material; wherein the chelating agent is sodium gluconate, and the reducing agent includes n-propanal; the molar ratio of sodium gluconate, divalent copper, and trivalent iron in the mixed reaction system is 2.5 × 10⁻⁶. -3 :1:1~1×10 -2 :1:
1.
2. The preparation method according to claim 1, characterized in that, Specifically, it includes: A copper source, a ferric source, and a surfactant are uniformly dispersed in a solvent, and then a chelating agent containing sodium gluconate solution is added to obtain a precursor solution. The precursor solution is uniformly mixed with alkali to obtain a suspension; The suspension and the reducing agent are uniformly mixed to obtain a mixed reaction system, and then the hydrothermal reaction is carried out.
3. The preparation method according to claim 2, characterized in that: An alkaline solution with an alkaline concentration of 0.125~0.5 g / mL is added in batches to the precursor solution at a rate of 1.5~3 mL / min while stirring is maintained to obtain the suspension.
4. The preparation method according to claim 1, characterized in that: The volume ratio of propionaldehyde to the total amount of divalent copper source and trivalent iron source in the mixed reaction system is 20:1 to 50:
1.
5. The preparation method according to claim 1, characterized in that: The molar ratio of copper, iron, and surfactant in the mixed reaction system is 1:1:1 to 1:1:
4.
6. The preparation method according to claim 2, characterized in that: The concentration of the sodium gluconate solution is 2.5 ~ 10 mmol / L.
7. The preparation method according to claim 1, characterized in that: The divalent copper source includes one or a combination of copper nitrate, copper sulfate, and copper chloride.
8. The preparation method according to claim 1, characterized in that: The trivalent iron source includes one or more combinations of ferric nitrate and ferric chloride.
9. The preparation method according to claim 1, characterized in that: The surfactant includes one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium oleate, and sodium lauryl sulfate.
10. The preparation method according to claim 1, characterized in that: The alkali includes one or more of sodium hydroxide and potassium hydroxide.
11. The preparation method according to claim 1, characterized in that: The hydrothermal reaction uses a mixed solvent, consisting of water and ethanol in a volume ratio of 1:4 to 1:
12.
12. The preparation method according to claim 1, characterized in that: The hydrothermal reaction takes 20 to 48 hours.
13. The preparation method according to claim 1, characterized in that: After the hydrothermal reaction is completed, the copper-ferrooxy material obtained from the reaction is post-treated. The post-treatment includes washing the copper-ferrooxy material with one or more of water, nitric acid, and ethanol, and then removing the water.
14. The copper ferrite material with an octahedral morphology obtained by the preparation method according to any one of claims 1-13.
15. The copper-ferrooxide material with an octahedral morphology according to claim 14, characterized in that: The copper-iron oxide material is an octahedral particle with a copper-iron ore crystal structure, orthorhombic 3R configuration, and cell parameters of a=3.0351Å, b=3.0351Å, c=17.166Å.
16. The copper ferrite material with an octahedral morphology according to claim 15, characterized in that: The particle size of the copper ferrite material is 2~5 μm.
17. The octahedral copper-ferrooxide material according to claim 15, characterized in that: The purity of the copper ferrite material is greater than or equal to 95%.
18. The octahedral copper-ferrooxide material according to claim 15, characterized in that: The crystallinity of the copper-ferrooxide material is greater than or equal to 60%.
19. The application of the octahedral copper-iron-oxygen material according to any one of claims 14-18 in photoelectrocatalysis.
20. A photocathode, characterized in that, The copper ferrite material with an octahedral morphology as described in any one of claims 14-18.
Citation Information
Patent Citations
Preparation method for octahedral CuFeO2 material
CN109879324A
Preparation method of CuFeO2 microcrystalline material of high-purity 3R delafossite structure
CN110395769A