A method for activating the soluble phosphorus and fluorine in phosphogypsum solidified by red mud

By utilizing the coupling effect of iron, aluminum, calcium, silicon, titanium and rare earth elements in red mud, the reaction between red mud and phosphogypsum is activated, and the soluble phosphorus and fluorine in phosphogypsum are solidified, thus solving the phosphogypsum pollution problem and realizing low-cost harmless treatment and industrial application.

CN118063124BActive Publication Date: 2026-11-24LONGYAN XINYIHAO ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410129297.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2026-11-24
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

Existing technologies are unable to effectively solidify soluble phosphorus and fluorine in phosphogypsum, leading to the risk of environmental pollution from phosphogypsum stockpiling. Furthermore, the high cost of treatment makes it difficult to achieve large-scale industrial-scale harmless treatment.

Method used

By utilizing the coupling effect of iron, aluminum, calcium, silicon, titanium and rare earth elements in red mud, the red mud is activated by adding acid or alkali, then added to phosphogypsum, and the pH value is adjusted to carry out a solidification reaction, so as to achieve complete fixation of soluble phosphorus and fluorine.

Benefits of technology

It achieves the harmless transformation of phosphogypsum into general solid waste, with a solidification rate of 99.5%, meeting environmental standards, and is low in cost, making it suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for activating red mud to solidify soluble phosphorus and fluorine in phosphogypsum. The method involves grinding red mud and then activating it with alkali or acid to obtain activated red mud. This activated red mud is then added to slurry-treated phosphogypsum, and the pH of the slurry is adjusted to 6-9 under stirring to carry out a solidification reaction. After the reaction, the mixture is filtered to obtain the final product. The amount of activated red mud added is 3-30% of the phosphogypsum mass. This method cleverly utilizes the coupled solidification effect of iron, aluminum, calcium, silicon, titanium, and rare earth elements in red mud on soluble phosphorus and fluorine in phosphogypsum, thereby transforming phosphogypsum from hazardous solid waste into general solid waste. This method achieves the technical objective of treating waste with waste, and has the advantages of simple process, good solidification effect, and low treatment cost, making it suitable for the large-scale industrial-scale harmless treatment of phosphogypsum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for solidifying soluble phosphorus and fluorine, specifically a method for activating red mud to solidify soluble phosphorus and fluorine in phosphogypsum, belonging to the fields of chemical and environmental protection technology. Background Technology

[0002] Red mud is a solid waste produced during the alumina production process. The composition of red mud varies depending on the alumina production process. The main components of Bayer process red mud are: SiO2 3–20%, CaO 2–8%, Al2O3 10–20%, Fe2O3 20–60%, Na2O 2–10%, TiO2 2–6%, and Re2O3 0.005–0.25%. The main components of sintering process red mud are: SiO2 20–23%, CaO 46–49%, Al2O3 5–7%, Fe2O3 7–10%, Na2O 2.0–2.2%, TiO2 1–7%, and Re2O3 0.01–0.5%. The main components of blended process red mud are similar to those of sintering process red mud. Red mud has a high pH value, with its leachate ranging from 10.3 to 13.0, and a fluoride content of 4.9 mg / L to 26.7 mg / L. According to GB 5058-85, the standard for pollution control of solid waste from non-ferrous metal industries, red mud with a pH value below 12.5 and a fluoride content of less than 50 mg / L is classified as general solid waste. In addition to iron, aluminum, calcium, silicon, and sodium, red mud also contains small amounts of titanium and rare earth elements.

[0003] Phosphogypsum is a byproduct of the wet-process phosphoric acid production process, and its main component is calcium sulfate. On average, 4-5 tons of phosphogypsum are produced for every ton of phosphoric acid produced using the wet-process method. Phosphogypsum inherits impurities from phosphate rock and the production process, such as P₂O₅, F, SiO₂, Al₂O₃, Fe₂O₃, and organic matter. The most problematic component is soluble phosphorus (H₂PO₄). - HPO4 2- ) and fluorine (F - The presence of soluble phosphorus and fluorine not only hinders the comprehensive utilization of phosphogypsum but also increases the risk of environmental pollution from phosphogypsum stockpiling. This is because phosphogypsum leachate is acidic and contains heavy metals in addition to phosphorus and fluorine; leaks can contaminate soil and surrounding water bodies. Therefore, the primary task in the harmless treatment of phosphogypsum is to remove soluble phosphorus and fluorine.

[0004] Currently, there are two main approaches to the harmless treatment of phosphogypsum: one is the transformation and utilization of phosphogypsum, and the other is to solidify the soluble phosphorus and fluorine in phosphogypsum, thus converting it from hazardous solid waste into general solid waste. While phosphogypsum, after washing and neutralization with lime, can be used as building materials, soil conditioners, and cement retarders, these products have low added value, and most wet-process phosphoric acid plants are located in remote areas far from major cities, resulting in high transportation costs and a lack of market competitiveness. However, once the soluble phosphorus and fluorine in phosphogypsum are solidified, it can become general solid waste, used as backfill material in abandoned mine shafts or as roadbed filler for road construction, achieving low-cost and rapid disposal of phosphogypsum.

[0005] According to the general waste definition standards (GB 18599-2020, GB 8978-1996), the treated phosphogypsum sample was ground to a particle size of less than 3 mm according to the toxicity leaching method (HJ 557—2010), then water was added at 10 times the dry weight and shaken for 8 hours, then allowed to stand for 16 hours and filtered. The resulting leachate should meet the following requirements: pH = 6-9, P ≤ 0.5 mg / L, F ≤ 10 mg / L.

[0006] There are three main methods for removing soluble phosphorus and phosphorus from phosphogypsum: thermal treatment, physical methods, and chemical methods. Thermal treatment uses high temperatures to decompose the organic matter in phosphogypsum, improving its whiteness. Simultaneously, it forces residual fluorine and chlorine to volatilize as hydrogen fluoride and hydrogen chloride, while converting soluble phosphorus into insoluble phosphates and pyrophosphates. However, thermal treatment is not only energy-intensive, but also incurs high costs for flue gas purification.

[0007] The physical method utilizes the differences in physical properties between calcium sulfate in phosphogypsum and phosphate rock decomposition residues and organic impurities, and uses methods such as ball milling, water washing, and flotation to separate soluble P and F.

[0008] Chemical methods, including acid leaching and alkali neutralization, aim to reduce the content of soluble phosphorus and fluorine in phosphogypsum. Physical and chemical methods can separate most of the soluble P and F in phosphogypsum, but the separation is incomplete, and the treated phosphogypsum cannot meet the standards for general solid waste. Some researchers have tried adding lime, cement, and various cementing materials such as PAM (polyacrylamide) to phosphogypsum to prevent the leaching of soluble P and F. However, with prolonged storage, the soluble P and F in the treated phosphogypsum will redissolve because the cement coating on the phosphogypsum particles is prone to cracking, and the organic cementing materials will degrade under the action of microorganisms. The solidification of soluble P and F in phosphogypsum has become a long-standing and unresolved problem in the phosphorus chemical industry. Summary of the Invention

[0009] To address the problems existing in the prior art, the present invention aims to provide a method for activating red mud to solidify soluble phosphorus and fluorine in phosphogypsum. This method ingeniously utilizes the coupled solidification effect of iron, aluminum, calcium, silicon, titanium, and rare earth elements in red mud on soluble P and F elements in phosphogypsum, thereby transforming phosphogypsum from hazardous solid waste into general solid waste. This method achieves the technical objective of treating waste with waste, and has the advantages of simple process, good solidification effect, and low treatment cost, making it suitable for the large-scale industrial harmless treatment of phosphogypsum.

[0010] To achieve the above-mentioned technical objectives, the present invention provides a method for activating red mud to solidify soluble phosphorus and fluorine in phosphogypsum. The red mud is ground and then activated by adding alkali or acid to obtain activated red mud. The activated red mud is added to phosphogypsum that has undergone slurry treatment, and the pH of the slurry is adjusted to 6-9 under stirring to carry out a solidification reaction. After the reaction is completed, the mixture is filtered to obtain the final product. The amount of activated red mud added is 3-30% of the mass of phosphogypsum.

[0011] As a preferred embodiment, the red mud is Bayer process red mud, sintered red mud, mixed process red mud, and a solidification agent formulated from chemical raw materials that has the same main components as the red mud.

[0012] As a preferred embodiment, the main components of the red mud are expressed in the following mass percentages: SiO2 3–23%, CaO 2–49%, Al2O3 5–50%, Fe2O3 7–60%, Na2O 2–10%, TiO2 1–10%, and Re2O3 0.001–1%. This invention is based on the coupled solidification effect of iron, aluminum, calcium, silicon, titanium, and rare earth elements in red mud on soluble phosphorus (P) and phosphorus (F) in phosphogypsum, thus completely fixing soluble P and F into the phosphogypsum. Therefore, the main components of the red mud and their proportions must strictly adhere to the above requirements.

[0013] As a preferred embodiment, the red mud is ground by dry grinding or wet grinding until the particle size is -200 mesh.

[0014] As a preferred embodiment, the red mud activation process is as follows: red mud is added to water at a solid-liquid ratio of 1:0.5-5 g / mL, and alkali is added to maintain the solution pH ≥ 13.5, and activated at 25-150℃ for 0.25-25 h.

[0015] As a preferred embodiment, the alkali is sodium hydroxide and / or potassium hydroxide.

[0016] As a preferred method, red mud is added to water at a solid-liquid ratio of 1:0.5-5 g / mL, and acid is added to maintain the pH of the solution at 0.25-2.5. The solution is then activated at 10-110℃ for 0.5-5 h.

[0017] As a preferred embodiment, the acid is at least one selected from sulfuric acid, hydrochloric acid, nitric acid, oxalic acid, and citric acid.

[0018] As a preferred embodiment, the slurry treatment process of the phosphogypsum is as follows: phosphogypsum is added to water at a solid-liquid ratio of 1:0.5-2.5 g / mL and stirred thoroughly to disperse.

[0019] As a preferred embodiment, the curing reaction conditions are: temperature of 20–50°C, pH of 6–9, and time of 1–5 hours.

[0020] As a preferred embodiment, the phosphogypsum undergoes phosphorus and fluorine enrichment and recovery treatment before the curing reaction. The process is as follows: the phosphogypsum is added to water or acidified water for washing, and the resulting wash water is neutralized and precipitated to obtain phosphorus and fluorine enriched residue.

[0021] As a preferred embodiment, the conditions for neutralization and precipitation are as follows: the pH of the wash water is adjusted to 6-8 using lime.

[0022] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0023] 1) The method provided by this invention ingeniously utilizes the coupled solidification effect of iron, aluminum, calcium, silicon, titanium and rare earth elements in red mud on soluble P and F elements in phosphogypsum, thereby transforming phosphogypsum from harmful solid waste into general solid waste; this method achieves the technical objective of treating waste with waste, and has the advantages of simple process, good solidification effect and low treatment cost, and is suitable for the harmless treatment of phosphogypsum on a large scale in industrial applications.

[0024] 2) The technical solution provided by this invention has excellent curing effect on both water-washed and unwashed phosphogypsum. The curing rate of P and F is ≥99.5%. According to the test, under the condition that the original phosphogypsum contains 0.18% soluble phosphorus and 0.26% soluble fluorine, after harmless treatment by the technical solution provided by this invention, the P content in the leachate is ≤0.5ppm and the F content is ≤10ppm, which meets the definition standard of general waste. Detailed Implementation

[0025] The present invention will be further described below with reference to embodiments. These embodiments are intended to illustrate the present invention and not to further limit the present invention.

[0026] To better illustrate the advantages of the technical solution of the present invention, the activation process of the activated red mud and the solidification agent prepared by using chemical raw materials according to the proportion of the main components of the red mud in the embodiments of the present invention is as follows:

[0027] 1) Red mud activated with acid

[0028] Using Bayer process red mud as raw material, the main components of the red mud are: SiO2 11%, CaO 6%, Al2O3 16%, Fe2O3 35%, Na2O 8%. The red mud is added to sulfuric acid at a solid-liquid ratio of 1:1 g / mL and heated to 105℃ for 2.5 h to activate it, thus obtaining the product.

[0029] 2) Red mud activated with alkali

[0030] Using red mud obtained by the mixed process as raw material, the main components of the red mud are: SiO2 11%, CaO 6%, Al2O3 16%, Fe2O3 35%, Na2O 8%; the mass ratio of red mud, sodium hydroxide and water is 1:1:1. After mixing evenly, the mixture is heated to 125℃ and activated for 1.5h to obtain the final product.

[0031] 3) Activation of curing agent with alkali

[0032] A curing agent is obtained by mixing bauxite containing 45% Al2O3, 9% SiO2, 11% Fe2O3, 2% TiO2 and a small amount of rare earth elements with quicklime containing 91% CaO at a mass ratio of 9:1. The curing agent, sodium hydroxide and water are mixed in a mass ratio of 1:2:1 and then heated to 125℃ for 2.5 hours to activate the mixture.

[0033] The phosphogypsum used in this embodiment of the invention contains 0.18% soluble phosphorus and 0.26% soluble fluorine.

[0034] The enrichment and recovery treatment of phosphorus and fluorine in the phosphogypsum is as follows: phosphogypsum is added to water at a solid-liquid ratio of 1:1 g / mL, stirred at room temperature for 1 hour, and filtered to obtain wash water with a pH of 2.1 and washed phosphogypsum. The soluble phosphorus and fluorine remaining in the washed phosphogypsum are then solidified with red mud. The resulting wash water is stirred and neutralized with lime to adjust the pH to 7.5, and filtered to obtain a neutralized liquid and phosphorus and fluorine enrichment residue. The phosphorus and fluorine enrichment residue is returned to be used as feedstock in the wet-process phosphoric acid production process, and the resulting neutralized liquid is returned to be used as wash water for phosphogypsum recycling.

[0035] Example 1

[0036] Take 100g of the above-mentioned washed phosphogypsum, add water at a solid-liquid ratio of 1:1 g / mL to form a slurry, then add 4.3g of acid-activated red mud, stir at 25℃, slowly add lime milk to adjust the pH to 8.5, maintain the solution pH ~8.5 and continue stirring for 3.5h, filter to obtain solidified phosphogypsum and its solidified liquid. Sample analysis of the solidified liquid: pH=8.6, P=0.2mg / L, F=9.3mg / L. This shows that the phosphogypsum treated with acid-activated red mud has been converted into general solid waste.

[0037] Example 2

[0038] 100g of the above-mentioned washed phosphogypsum was added to the treated liquid obtained in Example 1 for slurrying, followed by the addition of 3.5g of alkali-activated red mud. The pH was adjusted to 8.0 with dilute sulfuric acid, and the solution was maintained at pH ~8.0. The mixture was stirred at 45℃ for 1.5h, and then filtered to obtain solidified phosphogypsum and its solidified liquid. Analysis of the solidified liquid showed: pH = 7.8, P = 0.3mg / L, F = 8.9mg / L. This demonstrates that phosphogypsum treated with alkali-activated red mud can also be converted into general solid waste.

[0039] Example 3

[0040] Take 100g of the above-mentioned washed phosphogypsum, add it to the treated liquid obtained in Example 2 for slurrying, then add 5.2g of the alkali-activated solidifying agent, adjust the pH to 7.5 with dilute sulfuric acid, maintain the solution pH at 7.5, and continue stirring at 35℃ for 2.5h. Filter to obtain solidified phosphogypsum and its solidified liquid. Sample analysis of the solidified liquid: pH = 7.6, P = 0.1mg / L, F = 8.1mg / L. This shows that the solidifying agent prepared according to the proportion of the main components of red mud provided by this invention can also convert phosphogypsum into general solid waste.

[0041] Example 4

[0042] Take 30g of the unwashed phosphogypsum and add water at a solid-liquid ratio of 1:1 g / mL to slurry it. Then add 12.7g of acid-activated red mud, stir at 25℃, and slowly add lime milk to adjust the pH to 8.5. Maintain the solution pH at 8.5 and continue stirring for 3.5 hours. Filter to obtain solidified phosphogypsum and its solidified liquid. Sample analysis of the solidified liquid showed: pH = 8.4, P = 0.3 mg / L, F = 9.7 mg / L. This shows that unwashed phosphogypsum can be converted into general solid waste after treatment with acid-activated red mud.

[0043] Comparative Example 1

[0044] 100g of the above-mentioned washed phosphogypsum was added to water at a solid-liquid ratio of 1:1 g / mL to form a slurry. 30g of unactivated Bayer red mud (-200 mesh particle size) was added while stirring at room temperature. The pH was adjusted to 8.5 with dilute sulfuric acid. After maintaining the solution pH at ~8.5 for 0.5 hours, the solution was filtered to obtain solidified phosphogypsum and its solidified liquid. Analysis of the solidified liquid showed: pH = 8.4, P = 0.53 mg / L, F = 18.75 mg / L (>10 mg / L). This indicates that while unactivated red mud has some effect on solidifying soluble phosphorus and fluorine in phosphogypsum, it cannot meet the treatment standards for converting phosphogypsum into general solid waste.

Claims

1. A method for activating soluble phosphorus and fluorine in solidified red mud phosphogypsum, characterized in that: Red mud is ground and then activated by alkali or acid to obtain activated red mud. The activated red mud is added to phosphogypsum that has undergone slurry treatment, and the pH of the slurry is adjusted to 6-9 under stirring to carry out a solidification reaction. After the reaction is completed, it is filtered to obtain the final product. The amount of activated red mud added is 3-30% of the mass of phosphogypsum. The main components of the red mud, by mass percentage, include: SiO2 3~23%, CaO 2~49%, Al2O3 5~50%, Fe2O3 7~60%, Na2O 2~10%, TiO2 1~10%, and Re2O3 0.001~1%. The red mud activation process is as follows: add water to the red mud at a solid-liquid ratio of 1:0.5~5g / mL, add alkali to maintain the solution pH≥13.5, and activate at 25~150℃ for 0.25~25h. The red mud activation process is as follows: add water to the red mud at a solid-liquid ratio of 1:0.5~5g / mL, add acid to maintain the pH of the solution at 0.25~2.5, and activate at 10~110℃ for 0.5~5h.

2. The method for activating soluble phosphorus and fluorine in solidified red mud phosphogypsum according to claim 1, characterized in that: The red mud refers to Bayer process red mud, sintering process red mud, mixed process red mud, and solidification agents formulated from chemical raw materials that have the same main components as the red mud.

3. The method for activating soluble phosphorus and fluorine in solidified red mud phosphogypsum according to claim 1, characterized in that: The red mud is ground by dry grinding or wet grinding until the particle size is -200 mesh.

4. The method for activating soluble phosphorus and fluorine in solidified red mud phosphogypsum according to claim 1, characterized in that: The alkali is sodium hydroxide and / or potassium hydroxide.

5. The method for activating soluble phosphorus and fluorine in solidified red mud phosphogypsum according to claim 1, characterized in that: The acid is at least one of sulfuric acid, hydrochloric acid, nitric acid, oxalic acid, and citric acid.

6. The method for activating soluble phosphorus and fluorine in solidified red mud phosphogypsum according to claim 1, characterized in that: The slurry treatment process of the phosphogypsum is as follows: phosphogypsum is added to water at a solid-liquid ratio of 1:0.5~2.5g / mL and stirred thoroughly to disperse; the conditions for the curing reaction are: temperature of 20~50℃, pH of 6~9, and time of 1~5h.

7. The method for activating soluble phosphorus and fluorine in solidified red mud phosphogypsum according to claim 1, characterized in that: Before the curing reaction, the phosphogypsum undergoes a phosphorus and fluorine enrichment and recovery process, which involves adding the phosphogypsum to water or acidified water for washing. The resulting wash water is then neutralized and precipitated to obtain phosphorus and fluorine enriched residue.

8. The method for activating soluble phosphorus and fluorine in solidified red mud phosphogypsum according to claim 7, characterized in that: The conditions for neutralization and precipitation are as follows: the pH of the wash water is adjusted to 6-8 using lime.

Citation Information

Patent Citations

  • Efficient red mud fluorine removal agent and preparation method thereof

    CN114853296A

  • Method for in-situ stabilization of environmental pollutants in ardealite

    CN116573870A

  • Compositions and methods for reducing phosphorus and fluorine content in ardealite leachate

    CN117069230A