A method for smelting low-phosphorus stainless steel by using an electric furnace deep dephosphorization process
By using the electric furnace deep dephosphorization process, inexpensive raw materials and precise control of process parameters, the problems of high smelting cost and unstable quality of low-phosphorus stainless steel have been solved, realizing the production of low-phosphorus stainless steel with low cost and high quality, which meets the requirements of low carbon emission reduction.
Patent Information
- Application Number
- CN202410058079.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-16
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-16
AI Technical Summary
Existing low-phosphorus stainless steel smelting costs are high, the quality is unstable, and it does not meet the requirements for low-carbon emission reduction. Conventional smelting processes are difficult to control the composition, the phosphorus content fluctuates greatly, and the smelting success rate is low.
The process employs an electric furnace deep dephosphorization process, using inexpensive chromium-nickel scrap steel and chromium-nickel pig iron as raw materials. By precisely controlling the temperature of the electric furnace, optimizing the power supply curve and the timing of oxygen blowing, and combining oxygen blowing through the oxygen lance at the furnace door, the basicity and oxidizing properties of the slag are controlled, achieving stable deep dephosphorization within the electric furnace. The slag is then refined in an intermediate frequency furnace-AOD.
It significantly reduces smelting costs, stably controls phosphorus content at ≤0.005%, improves product quality, reduces carbon emissions, and meets the requirements for low-carbon emission reduction.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of stainless steel production technology, specifically relating to a method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process. Background Technology
[0002] In existing technologies, the smelting of low-phosphorus stainless steel generally adopts a production process of converter dephosphorized molten iron + medium-frequency furnace pre-melting liquid. The steelmaking raw materials of this process mainly use molten iron and expensive pure nickel, resulting in extremely high smelting costs for low-phosphorus stainless steel. Moreover, due to the difficulty in controlling the composition of conventional smelting processes, the phosphorus content fluctuates greatly, the smelting success rate is low, and the quality of low-phosphorus stainless steel is unstable. At the same time, using converters to smelt dephosphorized molten iron does not meet the requirements for low-carbon emission reduction.
[0003] Therefore, in order to complete the smelting and production of low-phosphorus stainless steel with guaranteed quality and low cost, technological innovation is necessary. Summary of the Invention
[0004] To address the aforementioned technical problems in the existing technology, the present invention provides a method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process, comprising the following steps:
[0005] S1. Electric furnace charging: Load the electric furnace with raw materials such as chromium-nickel scrap steel, chromium-nickel pig iron, and dust removal ash briquettes that meet the charging requirements.
[0006] S2. The electric furnace heats up, and the electric furnace starts arcing at level 4, with a voltage of 848V and a current of 66kA; after the electric furnace stabilizes, the voltage increases to 946V and the current increases to 73kA.
[0007] S3. Electric arc furnace oxygen blowing dephosphorization: When the electric arc furnace's power consumption per ton of steel reaches 300 kWh / t, oxygen blowing dephosphorization is performed through oxygen lances at the furnace door, with the oxygen blowing intensity controlled at 40-60 Nm. 3 / min, the binary basicity of the slag is controlled at 1.2 to 1.6, and the mass percentage content of FeO in the slag is controlled at 10 to 20%;
[0008] S4. In the medium-frequency furnace-AOD smelting process, steel is tapped from the electric furnace tapping port, and steel slag is mixed out. After the slag is removed by the slag removal station, the electric furnace molten steel is mixed into the medium-frequency furnace molten liquid to obtain stainless steel pre-melted liquid. Then, the mixed pre-melted liquid is added to AOD for steel refining to produce low-phosphorus stainless steel.
[0009] Furthermore, in the above-mentioned method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process, the temperature of the electric furnace smelting process is controlled at 1450–1570℃.
[0010] Furthermore, in the above-mentioned method for smelting low-phosphorus stainless steel using the electric furnace deep dephosphorization process, the carbon content in the molten metal inside the electric furnace is controlled to be greater than 0.9% by mass percentage.
[0011] The method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process of the present invention has the following advantages and beneficial effects:
[0012] Significantly reducing the smelting cost of low-phosphorus stainless steel: This invention develops an electric furnace deep dephosphorization process technology, which innovates the conventional smelting process of low-phosphorus stainless steel, "converter dephosphorized molten iron + medium frequency furnace - AOD", into "electric furnace deep dephosphorization + medium frequency furnace - AOD". The electric furnace uses a large amount of inexpensive chromium-nickel-containing materials to smelt low-phosphorus stainless steel, including scrap steel, chromium-nickel pig iron, etc., instead of mainly using molten iron and expensive pure nickel as in the existing technology. This can significantly reduce the smelting cost of low-phosphorus stainless steel and has obvious economic benefits.
[0013] Significantly reducing the phosphorus content of low-phosphorus stainless steel and significantly improving the quality of low-phosphorus stainless steel products: This invention fully utilizes electric furnace deep dephosphorization technology. Using scrap steel and chromium-nickel pig iron as raw materials in the electric furnace, through precise temperature control of the electric furnace, optimization of the electric furnace power supply curve and oxygen blowing timing, reasonable control of the alkalinity inside the electric furnace, and oxygen blowing through the oxygen lance at the furnace door for oxidation dephosphorization, stable deep dephosphorization can be achieved during the electric furnace smelting process. The phosphorus content of the molten metal inside the electric furnace can be stably controlled to ≤0.005%, thereby improving the quality of low-phosphorus stainless steel products.
[0014] Effectively reduces carbon emissions: This invention develops and uses electric furnace deep dephosphorization technology, which abandons the existing converter smelting dephosphorization process for molten iron. It can effectively reduce carbon emissions, meet the requirements of low carbon emission reduction, and has certain social benefits. Detailed Implementation
[0015] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0016] In order to complete the smelting and production of low-phosphorus stainless steel with high quality and low cost, this invention innovates the existing process and provides a method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process. The applicant, after analysis, believes that electric arc furnaces are the core equipment for smelting stainless steel. Using resources such as scrap steel and chromium-nickel pig iron to produce stainless steel has advantages such as low cost, low carbon emissions, environmental friendliness, and stable quality. Therefore, this invention develops an electric arc furnace deep dephosphorization process, innovating the conventional smelting process for low-phosphorus stainless steel, "converter dephosphorized molten iron + medium-frequency furnace - AOD," into "electric arc furnace deep dephosphorization + medium-frequency furnace - AOD." The electric arc furnace uses scrap steel and chromium-nickel pig iron as raw materials. Through precise temperature control, optimization of the electric arc furnace power supply curve and oxygen blowing timing, reasonable control of the furnace alkalinity, and the use of oxygen blowing through the furnace door oxygen lance and carbon steel red mud balls for oxidation dephosphorization, stable deep dephosphorization can be achieved during the electric arc furnace smelting process. The phosphorus content of the molten metal in the furnace can be stably controlled to ≤0.005%, improving the yield of low-phosphorus stainless steel and solving the technical problems of high cost, complex process routes, unstable quality, and non-compliance with low-carbon emission reduction requirements in existing technologies for low-phosphorus stainless steel.
[0017] Specifically, the method of smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process according to the present invention includes the following steps:
[0018] S1. Electric furnace charging: Load the electric furnace with raw materials such as chromium-nickel scrap steel, chromium-nickel pig iron, and dust removal ash briquettes that meet the charging requirements.
[0019] S2. The electric furnace is heating up. The electric furnace power supply curve is optimized as follows: when the electric furnace starts arcing at level 4, the voltage is 848V and the current is 66kA; after the electric furnace stabilizes, the voltage increases to 946V and the current increases to 73kA.
[0020] S3. Electric arc furnace oxygen blowing dephosphorization: The timing of electric arc furnace oxygen blowing is optimized as follows: when the electric arc furnace's power consumption per ton of steel reaches 300 kWh / t, oxygen blowing dephosphorization is performed through the oxygen lance at the furnace door, with the oxygen blowing intensity (i.e., oxygen flow rate) controlled at 40–60 Nm. 3 / min, the basicity inside the electric furnace is controlled as follows: the binary basicity of the slag (CaO / SiO2) is controlled at 1.2 to 1.6, and the FeO mass percentage content in the slag is controlled at 10 to 20%;
[0021] S4. In the medium-frequency furnace-AOD smelting process, steel is tapped from the electric furnace tapping port, and steel slag is mixed out. After the slag is removed by the slag removal station, the molten steel from the electric furnace is mixed into the molten steel in the medium-frequency furnace to obtain stainless steel pre-melted liquid. Then, the pre-melted liquid in the medium-frequency furnace is added to AOD for steel refining to produce low-phosphorus stainless steel.
[0022] Furthermore, in the method for smelting low-phosphorus stainless steel using the electric furnace deep dephosphorization process of the present invention, in order to use inexpensive high-phosphorus chromium-nickel materials, it is necessary to conduct thermodynamic theoretical research on the influencing factors and mechanisms of the electric furnace dephosphorization process. According to the Gibbs free energy curves of lime dephosphorization reaction, carbon-oxygen reaction, and chromium oxidation reaction, only in the lower temperature range of steelmaking temperature does phosphorus preferentially oxidize carbon (C) and chromium (Cr). Therefore, to satisfy the preferential oxidation of phosphorus, the electric furnace temperature should not be too high, which would lead to a decrease in the dephosphorization rate. However, if the electric furnace temperature is too low, the fluidity of the mother liquor and slag will be poor, which is also not conducive to dephosphorization. Through experiments on the main factors affecting the dephosphorization reaction, such as mother liquor temperature, carbon content, oxygen supply intensity, slag basicity, and oxidizing properties, it was determined that the target of phosphorus content ≤0.005% must be met. Therefore, in the method for smelting low-phosphorus stainless steel using the electric furnace deep dephosphorization process of the present invention, the electric furnace smelting process temperature is precisely controlled at 1450-1570℃, and the mass percentage content of carbon in the molten metal in the electric furnace is controlled to be greater than 0.9%.
[0023] In the method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process of the present invention, by studying the influence of oxygen potential and slag on the dephosphorization reaction and combining extensive production practice, the optimal oxygen supply intensity for dephosphorization was determined to be 40–60 Nm. 3 With a slag basicity ranging from 1.2 to 1.6 and an FeO content of 10% to 20%, efficient dephosphorization can be achieved.
[0024] In the method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process of the present invention, technical measures are adopted to prevent phosphorus accumulation after the electric furnace. Specifically, the conventional process route of the prior art involves transferring the dephosphorized molten iron from the converter to the molten iron in the medium-frequency furnace after steel is tapped from the medium-frequency furnace, and then adding AOD for steel smelting. The dephosphorization task is concentrated in the converter. In the present invention, however, the dephosphorization task is mainly carried out in the electric furnace. To prevent the problem of phosphorus accumulation caused by the mixing of electric furnace slag, for steel grades with extremely low phosphorus requirements, the slag is removed after tapping from the electric furnace and then added to the molten iron in the medium-frequency furnace. This solves the problem of phosphorus accumulation after the electric furnace and reduces the problem of pre-melted liquid sticking to the medium-frequency furnace.
[0025] The following describes in detail the method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process, in conjunction with comparative examples in the prior art and specific embodiments of the present invention.
[0026] Comparative Examples 1 and 2 in the prior art smelted low-phosphorus stainless steel S32205 using a conventional process with a 180t converter and a 50t medium-frequency furnace. Table 1 below lists the charge material structure and P content of the tapped steel in Comparative Examples 1 and 2:
[0027] Table 1. Material structure of S32205 smelting in a 180t BOF furnace + 50t medium-frequency furnace and P content of the tapped steel.
[0028] Furnace Molten iron, t Scrap steel, t High carbon ferrochrome, t Steel output P, ppm Comparative Example 1 134.8 5.8 50.2 112 Comparative Example 2 122.8 5.5 51.1 107
[0029] Examples 1, 2, and 3 of this invention follow the above-described method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process. A 160t electric furnace is used to smelt low-phosphorus stainless steel S32205 using inexpensive chromium-nickel-containing materials as the main raw material. Table 2 below lists the furnace charge structure and P content of the tapped steel in Examples 1, 2, and 3:
[0030] Table 2. Material structure of S32205 smelting in a 160t electric arc furnace and P content of tapped steel.
[0031] Furnace Total furnace load, t Scrap steel, t Chromium-nickel pig iron, t <![CDATA[Oxygen flow rate, Nm 3 / min]]> Steel output P, ppm Example 1 122.0 11.0 101.0 60 40 Example 2 121.5 9.8 101.4 60 45 Example 3 122.1 11.6 100.1 60 28
[0032] It can be clearly seen that the method of smelting low-phosphorus stainless steel using the electric furnace deep dephosphorization process of the present invention achieves a stable phosphorus content of ≤0.005% (50ppm) in the molten liquid of the electric furnace by performing deep dephosphorization during the melting process of the electric furnace.
[0033] In summary, compared with the prior art, the method of smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process of the present invention has the following advantages and beneficial effects:
[0034] (1) Significantly reduce the smelting cost of low-phosphorus stainless steel. This invention develops an electric furnace deep dephosphorization process technology, which innovates the conventional smelting process of low-phosphorus stainless steel, "converter dephosphorized molten iron + medium frequency furnace - AOD", into "electric furnace deep dephosphorization + medium frequency furnace - AOD". The electric furnace uses a large amount of inexpensive chromium-nickel-containing materials to smelt low-phosphorus stainless steel, including scrap steel, chromium-nickel pig iron, etc., instead of mainly using molten iron and expensive pure nickel as in the existing technology. This can significantly reduce the smelting cost of low-phosphorus stainless steel and has obvious economic benefits.
[0035] (2) Significantly reduce the phosphorus content of low-phosphorus stainless steel and significantly improve the quality of low-phosphorus stainless steel products. This invention makes full use of electric furnace deep dephosphorization technology. Using scrap steel and chromium-nickel pig iron as raw materials in the electric furnace, through precise temperature control of the electric furnace, optimization of the electric furnace power supply curve and oxygen blowing timing, reasonable control of the alkalinity in the electric furnace, and oxygen blowing with the oxygen lance at the furnace door for oxidation dephosphorization, stable deep dephosphorization can be achieved during the electric furnace smelting process. The phosphorus content of the molten metal in the electric furnace can be stably controlled to ≤0.005%, thereby improving the quality of low-phosphorus stainless steel products.
[0036] (3) Effectively reduce carbon emissions. This invention develops and uses electric furnace deep dephosphorization technology, which abandons the existing converter smelting dephosphorized molten iron process, effectively reducing carbon emissions, meeting the requirements of low carbon emission reduction, and having certain social benefits.
[0037] It should be noted that, in this document, the term "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, such that an article or device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such an article or device.
[0038] It should also be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the present invention.
Claims
1. A method for smelting low-phosphorus stainless steel using an electric furnace deep dephosphorization process, characterized in that, Includes the following steps: S1. Electric furnace charging: Load chromium-nickel scrap steel, chromium-nickel pig iron, and dust removal ash briquettes that meet the charging requirements into the electric furnace. S2. The electric furnace heats up, and the electric furnace starts arcing at level 4, with a voltage of 848V and a current of 66kA; after the electric furnace stabilizes, the voltage increases to 946V and the current increases to 73kA. S3, oxygen blowing dephosphorization in the electric furnace, the electric furnace ton steel power consumption reaches 300 kWh / t, and the oxygen blowing dephosphorization is carried out through the electric furnace door oxygen lance, the oxygen blowing intensity is controlled at 40-60 Nm / min, the slag binary basicity is controlled at 1.2-1.6, and the mass percentage content of FeO in the slag is controlled at 10-20%; 3 / min, the slag binary basicity is controlled at 1.2-1.6, and the mass percentage content of FeO in the slag is controlled at 10-20%; S4. Induction furnace-AOD smelting: steel is tapped from the electric furnace tapping port, and steel slag is mixed out. After the slag is removed by the slag removal station, the electric furnace molten steel is mixed into the induction furnace molten liquid to obtain stainless steel pre-melted liquid. Then, the mixed pre-melted liquid is added to AOD for steel refining to produce low phosphorus stainless steel. The electric furnace smelting process temperature is controlled at 1450~1570℃, and the carbon content in the molten metal inside the electric furnace is controlled to be greater than 0.9% by mass percentage. The method can stably control the phosphorus content of the molten metal in the electric furnace to ≤0.005%.
Citation Information
Patent Citations
Ultralow-temperature pressure vessel steel and smelting method thereof
CN115261709A
Process method for smelting duplex stainless steel at low cost
CN117344086A