Preparation method of high-strength high-conductivity copper-based graphene composite material
By using a method of ball milling and direct continuous extrusion after mixing the powder, the problems of high preparation cost and unstable performance of copper-based graphene composite materials have been solved. This method enables the low-energy consumption and short-process preparation of high-strength and high-conductivity copper-based graphene composite materials, which are suitable for power signal transmission lines in aerospace, automotive and rail transportation.
Patent Information
- Application Number
- CN202311739469.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-18
AI Technical Summary
Existing methods for preparing copper-based graphene composite materials suffer from problems such as high cost, unstable performance, poor batch stability and performance consistency, long production process, high energy consumption, and low yield. Furthermore, traditional methods are difficult to achieve large size and high conductivity.
By using a ball milling and powder mixing followed by direct continuous extrusion, copper-based graphene composite materials with (111) filament texture and extremely fine grains are prepared by mixing copper powder with a particle size of 50-200 mesh with few-layer graphene and rare earth elements and utilizing the inducing effect of graphene on copper grains during continuous extrusion. This avoids the traditional powder metallurgy and plastic deformation steps.
A high-strength, high-conductivity copper-based graphene composite material with uniform structure and stable performance was prepared. The tensile strength can reach more than 600 MPa, the conductivity is more than 95% IACS, and the energy consumption is reduced by more than 50%, realizing low-carbon and environmentally friendly large-scale production.
Smart Images

Figure CN118064749B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing a high-strength, high-conductivity copper-based graphene composite material, belonging to the field of metal composite materials. Background Technology
[0002] Copper and copper alloys are widely used in many industrial fields due to their excellent mechanical, corrosion-resistant, electrical, and thermal conductivity properties. With the rapid development of modern industry and the dramatic increase in application demands, the market has placed higher requirements on copper-based materials. However, the performance of single copper-based materials is limited; the tensile strength of pure copper is only about 200 MPa, far from meeting the requirements of modern power systems for conductor materials. Current methods to improve the performance of copper-based materials mainly include adding reinforcing phase materials, improving mechanical properties through plastic deformation, solid solution strengthening, and second-phase strengthening, but these methods also reduce the electrical conductivity of copper-based materials.
[0003] Copper has a high electron concentration, and graphene possesses extremely high carrier migration speed. Combining these two materials to form copper / graphene composites can achieve conductivity superior to pure copper and even silver. Copper / graphene composites have become a key development area in industry and academia, representing the future direction of high-conductivity materials. Currently, there are two main technical routes for preparing copper-based graphene composites: in-situ graphene growth on copper foil and material mixing. The in-situ graphene growth method uses CVD (chemical vapor deposition) to grow graphene on a copper foil substrate, and then hot-presses multiple layers of graphene copper foil to achieve interlayer metallurgical bonding, obtaining a high-conductivity material of a certain thickness. This method yields graphene with high coverage, good quality, and good orientation consistency within the matrix. However, its disadvantages include the limitation of current CVD technology, which prevents the growth of large-sized copper foil graphene, and the high cost of this preparation method. The main technical principle of the hybrid method is the physical mixing of copper (powder, granules, bulk, etc.) with graphene (or graphene oxide, etc.), followed by densification and shaping using methods such as hot isostatic pressing, casting, and electrical discharge sintering. However, due to the limitations of graphene dispersion uniformity, orientation consistency, and maximum effective addition amount in copper, the hybrid method still struggles to achieve high conductivity levels. Therefore, considering both material performance and manufacturing costs, improving upon the current limitations of copper-based graphene composite materials has become a hot research topic in this field. Summary of the Invention
[0004] The purpose of this invention is to provide a low-energy, short-process, continuous preparation method for high-strength and high-conductivity copper-based graphene composite materials. The copper-based graphene composite materials prepared by this method have uniform structure, stable performance, and a strength that can reach more than 3 times that of existing pure copper materials, while their conductivity is comparable to that of pure copper.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a high-strength, high-conductivity copper-based graphene composite material includes the following steps: (1) Copper powder with a particle size of 50-200 mesh is mixed with few-layer graphene and copper-rare earth intermediate alloy powder, and ball-milled to obtain a composite powder. The composite powder contains 0.1 wt%-1 wt% of graphene and 0.01 wt%-0.1 wt% of rare earth elements. (2) Preheat the continuous extrusion die to a temperature of 450~600℃, pour the composite powder obtained in step (1) into the extrusion cavity of the continuous extruder through the hopper at a pouring speed of 20~100g / s and an extrusion speed of 4~6 rpm to obtain a rod blank with a diameter of 8~12mm, and cool the rod blank. (3) The rod blank obtained in step (2) is subjected to multiple continuous extrusions. The extrusion die is heated to 350~500℃ and the extrusion passes are 4~10 to obtain a wire blank with a diameter of 2~3mm. The wire blank is then cooled.
[0006] In this invention, the process may also include step (4) multi-pass cold drawing, in which the wire blank obtained in step (3) is subjected to multi-pass cold drawing with a processing rate of 50-99%.
[0007] In this invention, since the continuous extrusion process is non-vacuum and at high temperatures, copper powder is easily oxidized by combining with oxygen in a non-vacuum environment. The addition of rare earth elements can prevent excessive air from being drawn in during the continuous extrusion process, control the oxygen content in the matrix, and thus improve the conductivity of the material. In step (1), the rare earth element is preferably lanthanum, scandium, or cerium.
[0008] Preferably, the copper powder has an irregular particle size and ≤10 graphene layers. Because excessively fine copper powder can cause slippage during continuous extrusion, failing to effectively refine the grains, while excessively coarse copper powder can lead to uneven powder mixing, graphene agglomeration, and coarse grains, the copper powder selected in this invention has a particle size of 50-200 mesh and an irregular shape.
[0009] Preferably, in step (1), zirconia grinding balls with a diameter of 5mm-10mm are used to fully grind the zirconia in a ball mill for 4-8 hours.
[0010] In step (2), since the mixed powder is prone to slippage during the extrusion deformation process on the extrusion roller, the extrusion speed should not be too fast, and the rotation speed should be controlled at 4~6 rpm.
[0011] Preferably, in steps (2) and (3), a mixture of alcohol and water is used for cooling, wherein the volume ratio of alcohol to water in the mixture is 1:3 to 1:5.
[0012] Preferably, in step (3), the total deformation of the multi-pass continuous extrusion is 90-95%.
[0013] The composite material obtained by the preparation method of the present invention has a (111) filament texture, the average grain size of the copper matrix is between 1 and 3 μm, the graphene size is between 10 and 30 nm, the tensile strength of the composite material is above 600 MPa, and the conductivity is above 95% IACS.
[0014] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention employs a method for preparing copper-based graphene composite materials by ball milling and direct continuous extrusion after powder mixing. This method avoids traditional powder metallurgy and plastic deformation processes, and features simple preparation process, high controllability, and continuous large-scale mass production. It overcomes the problems of poor batch stability and performance consistency of copper-based composite materials prepared by traditional powder metallurgy processes, as well as long production processes, high energy consumption, and low yield. This provides a new possibility for the preparation of high-performance copper-based composite materials.
[0015] 2. This invention utilizes the inductive effect of graphene on copper grains during continuous extrusion to induce preferred orientation of copper grains, thereby preparing a copper-based graphene composite material with extremely strong (111) filament texture and extremely fine grain size, in which graphene is uniformly dispersed at the nanoscale. (111) as a hard orientation can improve the strength of the material, while also being beneficial to electrical properties, and the final product is not limited by size.
[0016] 3. This invention uses copper powder as the matrix material and few-layer graphene as the reinforcing phase to prepare a copper-based graphene composite material with uniform structure, good electrical conductivity, high hardness, high tensile strength and good elongation. Compared with copper-based graphene composite materials prepared by traditional processes, the preparation method of this invention reduces energy consumption by more than 50%, helping to achieve the goal of low carbon and environmental protection. Attached Figure Description
[0017] Figure 1 The following is an electron backscatter diffraction (EBSD) pattern of the sample obtained in Example 1 of the present invention, wherein (a) is a grain pattern (average crystal size 2.27 μm), (b) is a grain orientation distribution pattern (mainly (111) type filament texture), (c) is a grain boundary distribution pattern, and (d) is a grain size distribution histogram.
[0018] Figure 2 This is a SEM scan image of the sample obtained in Example 1 of the present invention. Detailed Implementation
[0019] The present invention will be further described below with reference to the accompanying drawings and embodiments, but this does not imply a limitation on the scope of protection of the present invention.
[0020] This invention proposes a low-energy, short-process, continuous preparation method for high-strength, high-conductivity copper-based graphene composite materials. The preparation method includes the following steps: (1) powder mixing, mixing copper powder with a particle size of 50-200 mesh with 0.1 wt%-1 wt% of few-layer graphene and 0.01 wt%-0.1 wt% of ... copper powder with a particle size of 0.01 wt%-0.1 wt% of copper powder with a particle size of 50-200 mesh. (1) Mix wt% rare earth elements (added in the form of copper lanthanum, copper cerium, and copper scandium intermediate alloy powder), and fully ball mill in a ball mill with 5mm-10mm diameter zirconia ball milling beads for 4-8 hours to obtain composite powder; (2) Continuous extrusion: pour the composite powder into the extrusion cavity of the continuous extruder through the hopper at a pouring speed of 20-100g / s and an extrusion speed of 4-6 rpm to obtain a graphene copper composite rod blank with a diameter of 8-12mm; (3) Multi-pass continuous extrusion: select molds of different sizes and specifications according to the final use state, and perform multi-pass continuous extrusion on the rod blank. The extrusion mold heating temperature is 350-500℃, and the extrusion passes are 4-10 to obtain a wire blank with a diameter of 2-3mm (which can be a round or rectangular wire blank); (4) Multi-pass cold drawing: according to the use requirements, the wire blank can be cold drawn in multiple passes with a processing rate of 50-99%.
[0021] In step (1), the copper powder has a particle size of 50-200 mesh and an irregular shape, and the number of graphene layers is 1-10. Fine copper powder causes slippage during continuous extrusion, which cannot effectively refine the grains, while coarse copper powder leads to uneven powder mixing, graphene agglomeration, and coarse grains.
[0022] Furthermore, in step (1), 0.01 wt%-0.1 wt% of rare earth elements (lanthanum, cerium or scandium) need to be added. Since the continuous extrusion process is non-vacuum and the temperature is high, copper powder is easily oxidized by combining with oxygen in a non-vacuum environment. The addition of rare earth elements can prevent too much air from being drawn in during the continuous extrusion process and control the oxygen content in the matrix.
[0023] In step (2), without the conventional powder metallurgy and plastic processing method, the problems of poor batch stability and performance consistency, long production process, high energy consumption and low yield of copper-based composite materials prepared by traditional powder metallurgy processes are overcome. The copper-based composite materials prepared by the present invention have stable composition / structure / performance, tensile strength of more than 600 MPa, and conductivity of more than 95% IACS. The preparation process is simple, highly controllable, and can be continuously mass-produced. Compared with copper graphene composite materials prepared by traditional processes, the energy consumption is reduced by more than 50%.
[0024] In step (3), multi-pass large deformation continuous extrusion is used, with a total deformation of 90~95%. On the one hand, this is to further obtain the required sample size. On the other hand, multi-pass deformation can refine the grain size and graphene, while making the graphene uniformly dispersed on the matrix. Furthermore, the nanoscale graphene can further refine the copper matrix grains during the deformation process.
[0025] In step (4), since this type of material has the characteristics of high strength and high conductivity, it can be used as a power signal transmission line for aerospace, automobiles, rail transportation and other applications. Therefore, conductor wires of different sizes and specifications can be obtained by cold drawing according to the final application requirements.
[0026] Example 1 (1) Mix copper powder with a particle size of 50 mesh with 1 wt% of few-layer graphene (≤10 layers) and 0.1 wt% cerium (added in the form of copper-cerium intermediate alloy powder), and fully ball mill in a ball mill with 10 mm diameter zirconia ball milling beads for 8 hours to obtain composite powder; (2) First, preheat the continuous extrusion die to a temperature of 600℃. Pour the composite powder obtained in step (1) into the extrusion cavity of the continuous extruder through the hopper at a pouring speed of 100g / s and an extrusion speed of 6 rpm to obtain a graphene copper composite rod blank with a diameter of 12mm. After the rod blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol to water is 1:3). (3) Select molds of different sizes and specifications according to the final use state, and extrude the rod blank in step (2) in multiple passes. The extrusion mold heating temperature is 500℃, the extrusion passes are 10, the total deformation is 93.75%, and a wire blank with a diameter of 3mm is obtained. After the wire blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol and water is 1:3). (4) According to the usage requirements, the wire blank obtained in step (3) is subjected to multiple cold drawing passes, with a processing rate of 99%.
[0027] The performance indicators of the samples prepared using this embodiment are shown in Table 1. Figure 1 The EBSD images of the obtained samples are shown in (a) for grains (average crystal size 2.27 μm), (b) for grain orientation distribution (mainly (111) type filament texture), (c) for grain boundary distribution, and (d) for grain size distribution histogram. Figure 2 The SEM scan image of the obtained sample shows that the grain size is small and uniform, and the graphene size is between 10 and 30 nm, which is uniformly distributed on the substrate.
[0028] Example 2 (1) Mix copper powder with a particle size of 200 mesh with 0.1 wt% of few-layer graphene (≤10 layers) and 0.01 wt% of lanthanum (added in the form of copper-lanthanum intermediate alloy powder), and fully ball mill in a ball mill with 5 mm diameter zirconia ball milling beads for 4 hours to obtain composite powder; (2) First, preheat the continuous extrusion die to 450°C. Pour the composite powder obtained in step (1) into the extrusion cavity of the continuous extruder through the hopper at a pouring speed of 20g / s and an extrusion speed of 4 revolutions / min to obtain a graphene copper composite rod blank with a diameter of 8mm. After the rod blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol to water is 1:4). (3) Select molds of different sizes and specifications according to the final use state, and extrude the rod blank in step (2) in multiple passes. The extrusion mold heating temperature is 350℃, the extrusion passes are 4 passes, the total deformation is 93.75%, and a wire blank with a diameter of 2mm is obtained. After the wire blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol and water is 1:4). (4) According to the usage requirements, the wire blank obtained in step (3) is subjected to multiple cold drawing passes, with a processing rate of 94%.
[0029] The performance indicators of the samples prepared using this embodiment are shown in Table 1.
[0030] Example 3 (1) Mix copper powder with a particle size of 125 mesh with 0.5 wt% of few-layer graphene (≤10 layers) and 0.05 wt% of scandium (added in the form of copper-scandium intermediate alloy powder), and fully ball mill in a ball mill with 8 mm diameter zirconia ball milling beads for 6 hours to obtain composite powder; (2) First, preheat the continuous extrusion die to a temperature of 500℃. Pour the composite powder obtained in step (1) into the extrusion cavity of the continuous extruder through the hopper at a pouring speed of 50g / s and an extrusion speed of 5 revolutions / min to obtain a graphene copper composite rod blank with a diameter of 10mm. After the rod blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol and water is 1:5). (3) Select molds of different sizes and specifications according to the final use state, and extrude the rod blank in step (2) in multiple passes. The extrusion mold heating temperature is 400℃, the extrusion passes are 8, the total deformation is 91%, and a wire blank with a diameter of 3mm is obtained. After the wire blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol and water is 1:5). (4) According to the usage requirements, the wire blank obtained in step (3) is subjected to multiple cold drawing passes, with a processing rate of 50%.
[0031] The performance indicators of the samples prepared using this embodiment are shown in Table 1.
[0032] Example 4 (1) Mix copper powder with a particle size of 175 mesh with 0.2 wt% of few-layer graphene (≤10 layers) and 0.04 wt% of rare earth element cerium (added in the form of copper-cerium intermediate alloy powder), and fully ball mill in a ball mill with 6 mm diameter zirconia ball milling beads for 5 h to obtain composite powder; (2) First, preheat the continuous extrusion die to a temperature of 550℃. Pour the composite powder obtained in step (1) into the extrusion cavity of the continuous extruder through the hopper at a pouring speed of 70g / s and an extrusion speed of 6 rpm to obtain a graphene copper composite rod blank with a diameter of 9mm. After the rod blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol to water is 1:3). (3) Select molds of different sizes and specifications according to the final use state, and extrude the rod blank in step (2) in multiple passes. The extrusion mold heating temperature is 450℃, the extrusion passes are 8, the total deformation is 91.65%, and a wire blank with a diameter of 2.6mm is obtained. After the wire blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol and water is 1:3). (4) According to the usage requirements, the wire blank obtained in step (3) is subjected to multiple cold drawing passes, with a processing rate of 95%.
[0033] The performance indicators of the samples prepared using this embodiment are shown in Table 1.
[0034] Example 5 (1) Mix copper powder with a particle size of 100 mesh with 0.6 wt% of few-layer graphene (≤10 layers) and 0.06 wt% of rare earth element lanthanum (added in the form of copper lanthanum intermediate alloy powder), and fully ball mill in a ball mill with 8 mm diameter zirconia ball milling beads for 6 h to obtain composite powder; (2) First, preheat the continuous extrusion die to a temperature of 525℃. Pour the composite powder obtained in step (1) into the extrusion cavity of the continuous extruder through the hopper at a pouring speed of 60g / s and an extrusion speed of 8 rpm to obtain a graphene copper composite rod blank with a diameter of 12mm. After the rod blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol to water is 1:4). (3) Select molds of different sizes and specifications according to the final use state, and extrude the rod blank in step (2) in multiple passes. The extrusion mold heating temperature is 500℃, the extrusion passes are 6, the total deformation is 93.75%, and a wire blank with a diameter of 3mm is obtained. After the wire blank comes out of the continuous extruder, it is cooled in a cooling tank containing a mixture of alcohol and water (the volume ratio of alcohol and water is 1:4). (4) According to the usage requirements, the wire blank obtained in step (3) is subjected to multiple cold drawing passes, with a processing rate of 99%.
[0035] The performance indicators of the samples prepared using this embodiment are shown in Table 1.
[0036] Table 1 Performance indicators of samples prepared in Examples 1-5 As can be seen from the above embodiments, the present invention mixes copper powder of suitable particle size with few-layer graphene powder, and through continuous extrusion, uniformly disperses nano-sized graphene in the matrix. The uniformly dispersed nano-sized graphene plays a role in refining the grain size of the matrix during continuous extrusion, resulting in an average grain size of copper matrix between 1 and 3 μm (e.g., ...). Figure 1 (a) and Figure 1 (d) shows that the graphene size is between 10-30 nm (as shown in the figure). Figure 2 As shown in the figure, it plays a role in grain refinement and second-phase reinforcement, effectively improving the tensile strength of the material. The electrical conductivity of the material is comparable to that of pure copper, and the tensile strength can reach more than 600 MPa, which is more than 3 times that of pure copper.
[0037] This invention adds 0.01%-0.1% rare earth elements (lanthanum, scandium, cerium) to prevent excessive air from being entrained during continuous extrusion, control the oxygen content in the matrix, and thus improve the conductivity of the material.
[0038] During continuous extrusion, the inductive effect of graphene on copper grains is utilized to induce preferred orientation of the copper grains, thereby preparing a copper-based graphene composite material with an extremely strong copper (111) filament texture, such as... Figure 1 As shown in (b), (111) as a hard orientation can improve the strength of the material and is also beneficial to the electrical properties.
[0039] The preparation method of this invention is simple, highly operable, capable of continuous large-scale production, and exhibits good reproducibility. Compared with copper-graphene composite materials prepared by traditional processes, energy consumption is reduced by more than 50%, contributing to the achievement of low-carbon and environmentally friendly goals.
Claims
1. A method for preparing a high-strength, high-conductivity copper-based graphene composite material, characterized in that, Includes the following steps: (1) Mix copper powder with a particle size of 50-200 mesh with few-layer graphene and copper-rare earth intermediate alloy powder, and ball mill to obtain composite powder. The content of graphene in the composite powder is 0.1 wt%-1 wt%, and the content of rare earth elements is 0.01 wt%-0.1 wt%. The copper powder has an irregular shape and the number of graphene layers is ≤10. (2) Preheat the continuous extrusion die to a temperature of 450~600℃, pour the composite powder obtained in step (1) into the extrusion cavity of the continuous extruder through the hopper at a pouring speed of 20~100g / s and an extrusion speed of 4~6 rpm to obtain a rod blank with a diameter of 8~12mm, and cool the rod blank. (3) The rod blank in step (2) is subjected to multiple continuous extrusions, and the total deformation of the multiple continuous extrusions is 90~95%; the extrusion die heating temperature is 350~500℃, the extrusion passes are 4~10, and a wire blank with a diameter of 2~3mm is obtained, and the wire blank is cooled. (4) The wire blank obtained in step (3) is subjected to multiple cold drawing passes with a processing rate of 50-99%.
2. The preparation method of the high-strength, high-conductivity copper-based graphene composite material according to claim 1, characterized in that, The rare earth element is lanthanum, scandium, or cerium.
3. The preparation method of the high-strength, high-conductivity copper-based graphene composite material according to claim 1, characterized in that, In step (1), zirconium oxide grinding beads with a diameter of 5 mm to 10 mm are used to fully grind the material in a ball mill for 4 to 8 hours.
4. The method for preparing the high-strength, high-conductivity copper-based graphene composite material according to claim 1, characterized in that, In steps (2) and (3), a mixture of alcohol and water is used for cooling.
5. The method for preparing the high-strength, high-conductivity copper-based graphene composite material according to claim 4, characterized in that, The volume ratio of alcohol to water is 1:3 to 1:
5.
6. The method for preparing the high-strength, high-conductivity copper-based graphene composite material according to claim 1, characterized in that, The composite material has a (111) filament texture, the average grain size of the copper matrix is between 1 and 3 μm, the graphene size is between 10 and 30 nm, the tensile strength is above 600 MPa, and the conductivity is above 95% IACS.
Citation Information
Patent Citations
Preparation method for graphene reinforced copper-matrix electrical contact material