Exosome-loaded hydrogel and preparation method and application thereof
By preparing injectable hydrogels loaded with exosomes, the problem of liver regeneration after partial hepatectomy was solved, achieving effective liver regeneration and hemostasis, reducing the risk of liver failure, and improving the targeting and efficacy of exosomes.
Patent Information
- Application Number
- CN202410215305.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-27
AI Technical Summary
Liver regeneration after partial hepatectomy is a problem, especially the risk of liver failure due to rapid reduction in liver volume and limited regenerative capacity. Current intravenous exosome infusions have poor targeting and are easily cleared, making it difficult to effectively promote liver regeneration.
The method involves loading exosomes derived from mesenchymal stem cells onto an injectable hydrogel. The hydrogel is prepared by coating the surface of the liver resection stump after the procedure. The preparation method includes reacting hyaluronic acid with sodium periodate and mixing it with the exosomes, then adding carboxymethyl chitosan and lactobionic acid solution to form a hydrogel. The hydrogel exhibits good biocompatibility and adhesion.
Hydrogels can slowly release exosomes, promote liver regeneration, reduce the risk of postoperative liver failure, and have good tissue adhesion and hemostatic effects, thus improving the targeting and efficacy of exosomes in the liver.
Smart Images

Figure CN118079095B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of exosome hydrogel technology, and more particularly to a hydrogel loaded with exosomes, its preparation method and application. Background Technology
[0002] Partial hepatectomy is one of the main treatments for benign and malignant liver diseases. However, the rapid reduction in liver volume and the limited regenerative capacity of the liver after surgery are risk factors for liver failure and a major cause of high mortality rates after partial hepatectomy. Therefore, liver regeneration after partial hepatectomy is a pressing problem that needs to be solved in this field.
[0003] Previous studies have shown that exosomes derived from mesenchymal stem cells play an important role in liver regeneration. Among biomaterials, hydrogels have similar physicochemical and mechanical properties to the natural extracellular matrix, and possess advantages such as porous structure, water retention, biodegradability, cell growth support, and slow release, making them ideal carriers for transporting cells, drugs, growth factors, etc. in tissue engineering.
[0004] Currently, intravenous exosome infusion suffers from drawbacks such as poor targeting and easy clearance. In contrast, local administration can maintain a certain concentration of exosomes in the target area.
[0005] Therefore, using injectable hydrogels to load exosomes derived from mesenchymal stem cells and coating the surface of the liver resection stump with the injectable hydrogel is of great significance for liver regeneration, hemostasis, and prevention of postoperative adhesion. However, there is still little research on the application of hydrogels in liver regeneration. Therefore, it is necessary to provide an injectable hydrogel-loaded exosome to promote liver regeneration. Summary of the Invention
[0006] The purpose of this invention is to provide a hydrogel loaded with exosomes, its preparation method and application, to solve the problem of liver regeneration after partial hepatectomy.
[0007] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0008] This invention provides a method for preparing a hydrogel loaded with exosomes, comprising the following steps:
[0009] (1) Dissolve hyaluronic acid in water to obtain a hyaluronic acid solution;
[0010] (2) The hyaluronic acid solution obtained in step (1) is mixed with sodium periodate and reacted. After the reaction is completed, dialysis is performed, the dialysate is collected and dried to obtain oxidized hyaluronic acid.
[0011] (3) Dissolve the oxidized hyaluronic acid obtained in step (2) and mix it with exosomes derived from umbilical cord mesenchymal stem cells to obtain an oxidized hyaluronic acid exosome suspension.
[0012] (4) The oxidized hyaluronic acid exosome suspension obtained in step (3) is mixed with carboxymethyl chitosan aqueous solution and lactobionic acid aqueous solution to obtain a hydrogel loaded with exosomes.
[0013] Preferably, the molecular weight of the hyaluronic acid in step (1) is 1×10⁻⁶. 5 ~8×10 5 Da, the concentration of the hyaluronic acid solution is 8-12 mg / mL.
[0014] Preferably, the molar ratio of sodium periodate to hyaluronic acid in step (2) is 1 to 2:1, the reaction is carried out under light-protected conditions for 3 to 7 hours, the stirring speed during the reaction is 400 to 600 rpm, and a quencher is added after the reaction to terminate the reaction.
[0015] Preferably, the molecular weight cutoff of the dialysis bag used in step (2) is 3000-4000 Da; the drying is freeze drying, and the freeze drying temperature is -15 to -25°C, and the time is 28 to 36 hours.
[0016] Preferably, in step (3), the mass ratio of oxidized hyaluronic acid to exosomes derived from umbilical cord mesenchymal stem cells is 80-120:1-3, the mixing speed is 150-250 rpm, and the time is 3-7 min.
[0017] Preferably, the concentration of the carboxymethyl chitosan aqueous solution in step (4) is 2.5-3.5%, and the concentration of the lactobionic acid aqueous solution is 1.5-2.5%.
[0018] Preferably, the volume ratio of the oxidized hyaluronic acid exosome suspension to the carboxymethyl chitosan aqueous solution and the lactobionic acid aqueous solution in step (4) is 8-11:8-11:1.
[0019] This invention provides a hydrogel loaded with exosomes prepared according to the method described above.
[0020] The present invention also provides the application of the hydrogel in the preparation of products that promote liver regeneration.
[0021] The hydrogel loaded with exosomes provided by this invention has good biocompatibility, a certain degree of adhesion to liver tissue, and hemostasis. It can slowly release exosomes derived from mesenchymal stem cells, and thus can be used as a liver adjuvant in liver resection. This may reduce the occurrence of liver failure after liver surgery and provide the possibility for more effective application of exosomes in liver repair. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0023] Figure 1 The size of the exosomes in Experiment Example 1;
[0024] Figure 2 The microstructure of exosomes observed by TEM in Example 1;
[0025] Figure 3 The results of the detection of exosome surface membrane proteins in Experiment Example 1;
[0026] Figure 4 The effect of exosomes on hepatocyte proliferation and migration in Experiment Example 1;
[0027] Figure 5 This refers to the uptake of exosomes by hepatocytes in Experiment Example 1;
[0028] Figure 6 Day 1 in Experimental Example 2 ( Figure 6 (See above) and Day 7 ( Figure 6 The distribution of exosomes in the hydrogel is shown in the figure below.
[0029] Figure 7 The microstructure of the exosome-loaded hydrogel;
[0030] Figure 8 The gelling properties of the hydrogel in Experimental Example 2;
[0031] Figure 9 The injectability of the hydrogel in Experimental Example 2;
[0032] Figure 10 The self-healing properties of the hydrogel in Experimental Example 2;
[0033] Figure 11 The swelling properties of the hydrogel in Experimental Example 2;
[0034] Figure 12 This demonstrates the hemostatic effect of the hydrogel in Experimental Example 2.
[0035] Figure 13 The adhesion properties of the hydrogel to porcine skin tissue in Experiment Example 2;
[0036] Figure 14 The adhesion properties of the hydrogel to human skin in Experiment Example 2;
[0037] Figure 15 The adhesion properties of the hydrogel to the cross-section of the rat liver in Experiment Example 2;
[0038] Figure 16 The adhesion of cells to hydrogels of different concentrations in Experiment Example 2;
[0039] Figure 17 The results of live and dead staining in Experiment Example 2;
[0040] Figure 18 The hemolysis rate of the hydrogel in Experiment Example 2;
[0041] Figure 19 The relative cell viability was measured after treatment with the hydrogel extract in Example 2.
[0042] Figure 20 The release rate of exosomes in the hydrogel in Experiment Example 2;
[0043] Figure 21 This refers to the uptake of exosomes by hepatocytes after applying the treatment to the liver cross-section in different treatment groups in Experiment Example 3.
[0044] Figure 22 The pathological changes of vital organs in different treatment groups in Experiment 3;
[0045] Figure 23 The effect of different treatment groups on liver cell regeneration in Experiment 3. Detailed Implementation
[0046] This invention provides a method for preparing a hydrogel loaded with exosomes, comprising the following steps:
[0047] (1) Dissolve hyaluronic acid in water to obtain a hyaluronic acid solution;
[0048] (2) The hyaluronic acid solution obtained in step (1) is mixed with sodium periodate and reacted. After the reaction is completed, dialysis is performed, the dialysate is collected and dried to obtain oxidized hyaluronic acid.
[0049] (3) Dissolve the oxidized hyaluronic acid obtained in step (2) and mix it with exosomes derived from umbilical cord mesenchymal stem cells to obtain an oxidized hyaluronic acid exosome suspension.
[0050] (4) The oxidized hyaluronic acid exosome suspension obtained in step (3) is mixed with carboxymethyl chitosan aqueous solution and lactobionic acid aqueous solution to obtain a hydrogel loaded with exosomes.
[0051] In this invention, the molecular weight of the hyaluronic acid in step (1) is 1×10⁻⁶. 5 ~8×10 5 Da, preferably 2×105 ~6×10 5 Da, further preferably 2.5 × 10 5 ~4×10 5 Da, more preferably 3×10 5 Da; the concentration of the hyaluronic acid solution is 8-12 mg / mL, preferably 9-11 mg / mL, and more preferably 10 mg / mL.
[0052] In this invention, the molar ratio of sodium periodate to hyaluronic acid in step (2) is 1 to 2:1, preferably 1.2 to 1.8:1, and more preferably 1.5:1; the reaction is carried out under light-protected conditions for 3 to 7 hours, preferably 4 to 6 hours, and more preferably 5 hours; the stirring speed during the reaction is 400 to 600 rpm, preferably 450 to 550 rpm, and more preferably 500 rpm; and a quencher is added after the reaction to terminate the reaction.
[0053] In this invention, the quenching agent is preferably ethylene glycol.
[0054] In this invention, the molecular weight cutoff of the dialysis bag used in step (2) is 3000-4000 Da, preferably 3200-3800 Da, more preferably 3400-3600 Da, and even more preferably 3500 Da; the drying is freeze drying, the freeze drying temperature is -15 to -25°C, preferably -18 to -22°C, more preferably -20°C, and the time is 28 to 36 hours, preferably 30 to 34 hours, and even more preferably 32 hours.
[0055] In this invention, the mass ratio of oxidized hyaluronic acid to exosomes derived from umbilical cord mesenchymal stem cells in step (3) is 80-120:1-3, preferably 90-110:1-3, and more preferably 100:2; the mixing speed is 150-250 rpm, preferably 180-220 rpm, and more preferably 200 rpm, and the time is 3-7 min, preferably 4-6 min, and more preferably 5 min.
[0056] In this invention, the concentration of the carboxymethyl chitosan aqueous solution in step (4) is 2.5-3.5%, preferably 2.8-3.2%, and more preferably 3%; the concentration of the lactobionic acid aqueous solution is 1.5-2.5%, preferably 1.8-2.2%, and more preferably 2%.
[0057] In this invention, the volume ratio of the oxidized hyaluronic acid exosome suspension to the carboxymethyl chitosan aqueous solution and the lactobionic acid aqueous solution in step (4) is 8-11:8-11:1, preferably 9-10:9-10:1, and more preferably 9.5:9.5:1.
[0058] In this invention, the mixing method in step (4) is oscillation mixing, and the oscillation time is 5 to 20 seconds, preferably 10 to 18 seconds, and more preferably 15 seconds.
[0059] This invention provides a hydrogel loaded with exosomes prepared according to the method described above.
[0060] The present invention also provides the application of the hydrogel in the preparation of products that promote liver regeneration.
[0061] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0062] Example 1
[0063] The preparation method of exosomes derived from umbilical cord mesenchymal stem cells includes the following steps:
[0064] The umbilical cord samples were obtained from full-term newborns with no obvious infectious diseases, family history of genetic disorders, or other illnesses. The acquisition of the samples was ethical and in accordance with national laws and regulations, and informed consent was obtained from the donors.
[0065] Rinse the fresh umbilical cord with 75% alcohol for 30 seconds, then rinse twice with physiological saline. Cut the umbilical cord into 1cm long segments and place them in a 10cm petri dish. Next, cut the umbilical cord along the umbilical vein, remove one umbilical vein and two umbilical arteries, rinse again with physiological saline, and then cut into approximately 1mm pieces with scissors. 3 Small tissue pieces were carefully placed at the bottom of a T75 culture flask using tissue forceps. After incubating at 37°C for 3 hours, 15 mL of complete culture medium was added. Cell growth was observed on day 6, and the original culture medium was replaced on day 7. Cells were passaged when confluence reached 60–70%. For passage, cells were washed twice with PBS buffer, digested with 3 mL of trypsin for 2 min, centrifuged at 1000 rpm for 5 min after digestion, the supernatant was discarded, and the cells were resuspended and seeded in exosome-free serum-free medium. Cells were cultured until confluence reached 80–90%, the supernatant was collected, and the cells were passaged again.
[0066] Exosomes were extracted according to the kit instructions. First, cells were centrifuged at 3000g for 10 min to remove cells and some cell debris. The supernatant was collected and transferred to a new centrifuge tube, where it was centrifuged at 10000g for 15 min to further remove small debris and impurities. Then, the newly obtained supernatant was transferred in 15 mL increments to ultrafiltration centrifuge tubes (MWCO = 100 kDa), centrifuged at 5000 rpm for 15 min, and then concentrated to 250 μL. Next, 20 mL of the concentrated supernatant was weighed and gently mixed with 5 mL of ExoQuick-TC solution, and incubated at 4°C for 24 h. Subsequently, centrifugation at 10000g for 60 min was performed, and exosomes were observed precipitating on the centrifuge tube wall. The supernatant was gently aspirated. The obtained exosomes were resuspended in 200 μL of PBS, centrifuged again at 12000g for 2 min, and then stored at -80°C for later use.
[0067] Example 2
[0068] A method for preparing a hydrogel loaded with exosomes, comprising the following steps:
[0069] (1) Take 1.0g of hyaluronic acid (HA, Shanghai Aladdin Biochemical Technology Co., Ltd., molecular weight 3×10⁻⁶). 5 Da) was dissolved in 100 mL of double-distilled water to obtain a hyaluronic acid solution with a concentration of 10 mg / mL.
[0070] (2) Add 0.80 g of sodium periodate (NaIO4) to the hyaluronic acid solution obtained in step (1), wherein the molar ratio of NaIO4 to HA is 1.5:1. Mix and react for 5 h in the dark at room temperature (25℃) with a stirring speed of 500 rpm. After the reaction, add 2 mL of ethylene glycol to terminate the reaction for 1 h. Dialyze using a dialysis bag with a cutoff of 3500 Da for 3 days, changing the solution every 4 hours until there is no periodate in the dialysate (the method for detecting periodate is: add 0.5 mL of dialysate to 0.5 mL of 1% silver nitrate solution; if there is no precipitate, it indicates that there is no periodate). After dialysis, quench the dialysate with liquid nitrogen and then quickly place it in a freeze dryer and freeze dry at -20℃ for 32 h to obtain oxidized hyaluronic acid (OHA).
[0071] (3) Weigh 0.1g of the oxidized hyaluronic acid prepared in step (2) and add it to 5mL of 1×PBS buffer solution to dissolve it. Add 2mg of the exosomes derived from umbilical cord mesenchymal stem cells prepared in Example 1 and stir in a magnetic stirrer at 200rpm for 5min to obtain an oxidized hyaluronic acid exosome suspension with a mass fraction of 2%.
[0072] (4) Dissolve carboxymethyl chitosan powder (90% deacetylation, 80% carboxymethyl) and lactobionic acid powder in PBS buffer to obtain 3% carboxymethyl chitosan and 2% lactobionic acid aqueous solution. Mix 475 μL of 3% carboxymethyl chitosan and 50 μL of 2% lactobionic acid aqueous solution with 475 μL of 2% oxidized hyaluronic acid exosome suspension obtained in step (3) by shaking for 10 s. After standing for 30 s to form a gel, the hydrogel loaded with exosomes (CMC / OHA / LA-Exos) is obtained.
[0073] Simultaneously, a hydrogel without exosomes was prepared by shaking 475 μL of 3% carboxymethyl chitosan and 50 μL of 2% lactobionic acid aqueous solution for 10 s, followed by standing for 30 s to form a gel, thus obtaining the hydrogel without exosomes (CMC / OHA / LA).
[0074] Example 1: Characterization and function of exosomes
[0075] 1. Exosome diameter
[0076] 30 μL of the exosome stock solution prepared in Example 1 was diluted to 1 mL and then analyzed for particle size using a nanoparticle tracking analyzer. The NTA results are as follows: Figure 1 As shown, the diameter of the exosomes is approximately 87.1 nm.
[0077] 2. Exosome structure
[0078] After fixing the exosome solution with 2.5% glutaraldehyde solution overnight at 4°C, 10 μL was dropped onto a copper grid and allowed to stand at room temperature for 5 min. The liquid was then absorbed by filter paper. Staining solution (saturated uranium acetate-acetic acid solution) was added to the copper grid and stained for 1 min, then the liquid was absorbed by filter paper. ddH₂O was added to the copper grid and allowed to stand at room temperature for 5 min, then the liquid was absorbed by filter paper; this process was repeated once. The mixture was then dried at room temperature and observed and photographed using a TEM scanner. The TEM results are as follows: Figure 2 As shown, exosomes have a clear membrane structure resembling a saucer or cup, with clear edges, and are evenly distributed without aggregation.
[0079] 3. Detection of exosome markers
[0080] After exosome concentration detection, 20 μg of exosomes (with an equal volume of culture supernatant as a control) were added to 5×SDS-PAGE Loading Buffer and mixed thoroughly. The mixture was then heated at 95℃ for 5 min. SDS-PAGE electrophoresis: Acrylamide separating gel concentration was 12%. The supernatant from the above heating treatment was added to each sample well, and electrophoresis was performed (70V / 30 min, 120V / 60 min). Transfer: Wet transfer at 250 mA constant current for 90 min. Blocking: Block with 5% skim milk powder at room temperature for 1 h. Incubation with primary antibody: The antibody was diluted with 5% skim milk powder (antibody diluted 1000 times) and incubated overnight at 4℃. Incubation with secondary antibody: The primary antibody was aspirated, and the membrane was washed 3 times with TBST (5 min / wash). HRP-labeled secondary antibody (1:5000) was added, and the membrane was incubated at room temperature for 1 h. Imaging: After secondary antibody incubation, the membrane was washed 3 times with TBST (5 min / wash) and then imaged using ELC chemiluminescence buffer. Results of exosome surface membrane protein detection are as follows Figure 3 As shown, exosome markers CD63, CD9, and ALix are positively expressed.
[0081] 4. Effects of exosomes on hepatocyte proliferation and migration
[0082] Rat BRL-3A hepatocytes (purchased from the Cell Bank of the Chinese Academy of Sciences Type Culture Collection) were processed at a concentration of 1.6 × 10⁻⁶. 6 Cells were seeded per well in 24-well plates. After complete cell adhesion, exosomes were added at concentrations of 0, 5 μg / mL, 50 μg / mL, and 100 μg / mL, respectively, for intervention. Scratches were then made in each well. Images were taken under a microscope at 0, 12, and 24 hours to observe the healing status of hepatocytes in each treatment group and calculate the healing degree. Healing degree = (S0 - S2) / (S2) t ) / S0×100%, where S0 is the initial area of the hepatocytes, S t The area of liver cells at different times when photographed.
[0083] The results are as follows Figure 4 As shown, the results indicate that the healing ability increases with increasing doses of different concentrations of exosomes, suggesting that exosomes have a certain dose-dependent effect.
[0084] 5. Hepatocyte uptake of exosomes
[0085] Rat BRL-3A hepatocytes were divided into 5×10 3Cells were seeded per well in 24-well plates and high-glucose DMEM medium was added. After 12 hours of cell adhesion, 50 μg of exosomes were added. After 24 hours, the medium was removed, 4% paraformaldehyde was added, and the cells were incubated at room temperature for 15 minutes. The cells were then washed three times with PBS buffer, 3 minutes each time. After washing, DAPI was added for fixation for 5 minutes, followed by two more washes with PBS buffer. Images were taken under an inverted fluorescence microscope. Results are shown below. Figure 5 As shown, exosomes can be effectively taken up by BRL-3A cells.
[0086] Experimental Example 2: Properties of Hydrogels
[0087] 1. Stability
[0088] The distribution of exosomes in the hydrogel on days 1 and 7 was observed under a confocal microscope, and the results are as follows: Figure 6 As shown, it was found on day 1 ( Figure 6 (See above) and Day 7 ( Figure 6 The distribution of exosomes can be observed in the figure below, indicating that the hydrogel loaded with exosomes has good stability.
[0089] 2. Microscopic morphology
[0090] The microstructure of the freeze-dried hydrogel sample CMC / OHA / LA-Exos was evaluated using scanning electron microscopy, and the internal morphology and structure of the dried hydrogel after gold sputtering were analyzed. The experimental results are as follows: Figure 7 As shown, the hydrogel exhibits a porous microstructure with interconnected pores, providing stability. The pore size varies between 60 μm and 200 μm; smaller pores facilitate cell adhesion, growth, and removal of metabolic waste, while pores larger than 100 μm promote angiogenesis and endogenous tissue growth. This multi-sized porous structure enhances the hydrogel's porosity and mechanical stability, benefiting cell survival, proliferation, cell-cell interactions, and hydrogel-tissue compatibility. Furthermore, a large number of exosomes were observed adhering to the hydrogel, indicating their ability to be stored within the hydrogel without degradation.
[0091] 3. Gelatinizing properties, injectability, self-healing properties, and swelling effect.
[0092] Gelation property: The hydrogel loaded with exosomes prepared by mixing oxidized hyaluronic acid exosome suspension with carboxymethyl chitosan aqueous solution and lactobionic acid aqueous solution in Example 2 can gel within 30-40 seconds. Figure 8 ).
[0093] Injectability: 475 μL of a 2% oxidized hyaluronic acid exosome suspension, 475 μL of a 3% carboxymethyl chitosan suspension, and 50 μL of a 2% lactobionic acid aqueous solution were drawn into a 10 mL syringe and injected through a needle, indicating that the hydrogel has certain injectability properties. Figure 9 ).
[0094] Self-healing property: When the hydrogel was prepared into a heart shape and then cut in the middle, it was found that the gel could heal itself after 1 hour, indicating that the gel has a certain self-healing property. Figure 10 ).
[0095] Swelling effect: Freeze-dried CMC / OHA / LA and CMC / OHA / LA-Exos hydrogels (m0) were immersed in 5 mL centrifuge tubes containing 2 mL of phosphate-buffered saline (PBS, pH 7.4) and placed in a 37°C incubator. The tubes were removed from the PBS at time points (T = 30 min, 2 h, 4 h, 6 h, and 12 h), excess PBS was wiped off, and the weight of each sample (m1) was recorded. The swelling rate was calculated using the following formula: Swelling rate (%) = (m1 - m0) / m0 × 100%. Experimental results are as follows: Figure 11 As shown, CMC / OHA / LA and CMC / OHA / LA-Exos hydrogels exhibit good swelling behavior, and swelling equilibrium can be achieved within 360 min.
[0096] 3. Hemostatic effect
[0097] 200 μL of heparinized whole blood was added to an ampoule, followed by 200 μL of a 3% carboxymethyl chitosan lactobionic acid solution and 200 μL of a 2% oxidized hyaluronic acid mixture. After 1 minute, the hydrogel formed and exhibited hemostatic properties. Figure 12 ).
[0098] 4. Tissue adhesion properties
[0099] To verify the tissue adhesion properties of the hydrogel, a torsion test was conducted on pigskin. The hydrogel was injected into the surface of the pigskin. When torsional stress was applied in different directions, the CMC / OHA / LA hydrogel remained tightly adhered to the pigskin and remained intact. Figure 13 This demonstrates the tissue's adhesive and deformable capabilities. This strong tissue adhesion can be attributed to the synergistic effect of Schiff base bonds between aldehydes and amino groups in the tissue, as well as the electrostatic interaction between protonated amino groups and cell membrane phospholipids. Furthermore, injecting the hydrogel into human skin ( Figure 14 ) and rat liver cross section ( Figure 15 It still has strong tissue adhesion properties.
[0100] 5. Biocompatibility
[0101] The biocompatibility of the hydrogel was verified through cell adhesion, live / dead staining, hemolysis, and cytotoxicity assays.
[0102] 1) Cell adhesion
[0103] Different concentrations of OHA hydrogel were seeded into 6-well plates. After standing for 30 minutes to form a gel, BRL-3A cells were seeded into the gel and cultured for 24 hours. Cells were then fixed with 95% ethanol solution for 30 minutes, followed by washing three times with PBS, staining with 0.01% acridine orange, and observing cell morphology, number, and growth status under a fluorescence microscope 10 minutes later. Experimental results are as follows: Figure 16 As shown, the results indicate that cells exhibit certain adhesion properties in solutions of different concentrations of oxidized hyaluronic acid (OHA), but the adhesion properties are relatively poor in 4% OHA solutions.
[0104] 2) Live and dead staining
[0105] BRL-3A cells were divided into 1×10 6 Cells were seeded at a concentration of [number] cells / well in 6-well plates. After cell adhesion, hydrogel extraction buffer was added, and the cells were cultured for 24 hours. Live and dead cell staining was then performed. The working solutions for the live and dead cell staining were prepared by diluting reagent A (Calcein-AM) 4 μL and reagent B (PI) 5 μL 10-fold with dye dilution buffer (solution C: assay buffer). A 1:9 assay buffer was prepared. Then, appropriate amounts of serum-free culture medium were mixed with the diluted solutions A and B, and stored in the dark for immediate use. Cells were then washed with PBS, and 1 mL of the working solution was taken. The cells were incubated at 37°C in the dark for 20 min, and the staining solution was discarded. Finally, the cells were washed three times with PBS. The results were observed under a fluorescence microscope as shown below. Figure 17 As shown, no obvious cell death was observed.
[0106] 3) Hemolysis test
[0107] Blood was collected from the abdominal aorta of rats into an anticoagulant tube and centrifuged at 1000 rpm for 10 min. Red blood cells were then collected and diluted with physiological saline to 0.17% (v / v). The precursor solution of the hydrogel material was added to the diluted blood (1 mL) and incubated at 37℃ for 1 h. The mixture was then centrifuged at 2000 rpm for 5 min, and 200 μL of the supernatant was collected. The absorbance at 545 nm was measured using a microplate reader. The distilled water treatment group served as the positive control (100% hemolysis), and physiological saline served as the negative control. The hemolysis rate (HR, %) was calculated using the following formula: HR(%) = (Ds-NS) / (Ds-DW) × 100, where Ds, NS, and DW refer to the absorbance of the sample, physiological saline, and distilled water, respectively. The measurement results are as follows: Figure 18 As shown, the results were all less than 2%, indicating that no hemolysis occurred in any of the sample groups.
[0108] 4) Cytotoxicity assay
[0109] BRL-3A cells were divided into 5 × 10 3 Cells were seeded at a concentration of [number] cells / well in 96-well plates and cultured for 24 h, 48 h, and 72 h using 10%, 50%, and 100% hydrogel extract, respectively. The OD value of the hydrogel was then observed at 450 nm using a microplate reader, and the relative cell viability was calculated as control group / experimental group. Results are as follows: Figure 19 As shown, the relative survival rates of cells at 24h, 48h, and 72h were all greater than 1, confirming that no obvious cytotoxicity was observed.
[0110] 6. The effect of hydrogels in releasing exosomes
[0111] At 37℃, 100 μg of exosome hydrogel loaded with PKH-26 was immersed in a centrifuge tube containing 10 mL of PBS. 500 μL of the liquid was aspirated daily into a 96-well plate, and fluorescence intensity was detected using a fluorescence microplate reader (excitation at 480 nm, emission at 520 nm). 500 μL of PBS was then added, and the results were monitored daily until day 10. The results showed that exosomes were released from the hydrogel for 10 days. Figure 20 ).
[0112] Experimental Example 3
[0113] The purpose of this study is to investigate the biocompatibility and effects on liver regeneration of the hydrogel group, the exosome group, and the hydrogel + exosome group.
[0114] 1. The effect of hepatocytes on the uptake of exosomes after application to a liver cross-section
[0115] After hepatectomy in rats, hydrogels without exosomes (Hydrogel), exosomes (EXos), and PKH-26-labeled hydrogels loaded with exosomes (Hydrogel+EXos) were applied to the rat liver sections. One day post-surgery, the rats were sacrificed, and the uptake of exosomes by the liver was detected by immunofluorescence. Results are as follows: Figure 21 As shown in the figure (scale bar is 10μm), the yellow arrows point to exosomes in the cytoplasm, indicating that exosomes can be effectively taken up by rat hepatocytes.
[0116] 2. Biocompatibility
[0117] Eighteen 8-week-old male rats (weighing 180g-220g) were randomly divided into three groups: CMC / OHA / LA hydrogel group, exosome group, and CMC / OHA / LA hydrogel + exosome group. The surgical procedure for 70% of liver resections complied with ethical requirements. After skin preparation, a midline incision of approximately 3-4 cm was made in the upper abdomen. The abdominal cavity was accessed layer by layer, and the xiphoid process root was exposed by dissection. The ligaments surrounding the left lobe of the liver were severed using microsurgical scissors, and the liver was freed to its pedicle. A 4-0 suture was placed at the base of the pedicle, and after complete ligation, the left lobe was removed using ophthalmic scissors. When removing the middle lobe, the resection site was kept appropriately away from the inferior vena cava to avoid damage to the inferior vena cava, which could lead to bleeding and rat death. Subsequently, 5% of the right lobe of the liver was removed, resulting in a liver section on which 400 μL of exosome-loaded hydrogel was applied. After checking for residual liver tissue and confirming the absence of active bleeding in the abdominal cavity, the abdominal wall was intermittently sutured, the skin was continuously sutured, bloodstains were wiped away, and the surgical incision was disinfected to conclude the surgery. One week post-surgery, the rats were sacrificed, and the heart, liver, spleen, lungs, and kidneys of each group were harvested for HE staining to observe for damage to vital organs. Results are as follows: Figure 22 As shown, there were no obvious changes in the microstructure of the major organs in each group, and the hydrogel did not show obvious toxicity to the vital organs.
[0118] 3. Liver cell regeneration
[0119] To further investigate the role of exosome-loaded hydrogels in liver regeneration after hepatectomy, immunohistochemical analysis was performed. PCNA was used as the primary antibody, followed by incubation with a secondary antibody, and then treatment with horseradish peroxidase and 3,3'-diaminobenzidine solution. Finally, tissue sections were counterstained with hematoxylin. PCNA is a biological marker for proliferating cells. Results are as follows: Figure 23 As shown, the number of proliferation-labeled positive cells was significantly increased in the exosome-loaded hydrogel treatment group, indicating that cell replication was active in the regenerated tissue.
[0120] As can be seen from the above embodiments, the present invention provides a hydrogel loaded with exosomes, its preparation method, and its application. The hydrogel loaded with exosomes prepared by the present invention has good biocompatibility, exhibits a certain degree of adhesion to liver tissue, and can stop bleeding, making it a promising dressing for promoting liver regeneration after liver resection.
[0121] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a hydrogel loaded with exosomes to promote liver regeneration, characterized in that, Includes the following steps: (1) Dissolve hyaluronic acid in water to obtain a hyaluronic acid solution; (2) The hyaluronic acid solution obtained in step (1) is mixed with sodium periodate and reacted. After the reaction is completed, dialysis is performed, the dialysate is collected and dried to obtain oxidized hyaluronic acid. (3) Dissolve the oxidized hyaluronic acid obtained in step (2) and mix it with exosomes derived from umbilical cord mesenchymal stem cells to obtain an oxidized hyaluronic acid exosome suspension; (4) The oxidized hyaluronic acid exosome suspension obtained in step (3) is mixed with carboxymethyl chitosan aqueous solution and lactobionic acid aqueous solution to obtain a hydrogel loaded with exosomes; The mass ratio of oxidized hyaluronic acid to exosomes derived from umbilical cord mesenchymal stem cells in step (3) is 80-120:1-3; In step (4), the concentration of the carboxymethyl chitosan aqueous solution is 2.5-3.5%, and the concentration of the lactobionic acid aqueous solution is 1.5-2.5%. The volume ratio of the oxidized hyaluronic acid exosome suspension to the carboxymethyl chitosan aqueous solution and the lactobionic acid aqueous solution in step (4) is 8~11:8~11:
1.
2. The method as described in claim 1, characterized in that, The hyaluronic acid in step (1) has a molecular weight of 1×10⁻⁶. 5 ~8×10 5 Da, the concentration of the hyaluronic acid solution is 8~12 mg / mL.
3. The method as described in claim 2, characterized in that, In step (2), the molar ratio of sodium periodate to hyaluronic acid is 1~2:
1. The reaction is carried out under light-protected conditions for 3~7 hours. The stirring speed during the reaction is 400~600 rpm. After the reaction, a quencher is added to terminate the reaction.
4. The method as described in claim 3, characterized in that, The molecular weight cutoff of the dialysis bag used in step (2) is 3000~4000 Da; the drying is freeze drying, the freeze drying temperature is -15~-25℃, and the time is 28~36h.
5. The method as described in claim 4, characterized in that, The mixing speed in step (3) is 150~250 rpm and the time is 3~7 min.
6. A hydrogel loaded with exosomes prepared according to any one of claims 1 to 5.
7. The use of the hydrogel of claim 6 in the preparation of products that promote liver regeneration.
Citation Information
Patent Citations
Exosome sustained release system and construction method and application thereof
CN110123842A