Preparation method of PS / PMMA biomimetic super-hydrophobic membrane for oil-water separation
By imprinting a biomimetic porous membrane onto a PI membrane and modifying it with a PMMA-b-PDMS-b-PS superhydrophobic compound, combined with carbon nanotubes, a PS/PMMA biomimetic superhydrophobic membrane with high mechanical strength and high oil-water separation efficiency was prepared, solving the problem of insufficient strength and efficiency of existing membrane materials.
Patent Information
- Application Number
- CN202410353172.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Existing superhydrophobic composite membranes have low mechanical strength and low oil-water separation efficiency, making it difficult to meet the increasingly demanding requirements for oil-water separation.
A PS/PMMA biomimetic superhydrophobic membrane preparation method was adopted, which involves imprinting a biomimetic porous membrane on a PI membrane and modifying the surface with a PMMA-b-PDMS-b-PS superhydrophobic compound, combined with carbon nanotubes to improve mechanical strength and hydrophobic properties.
It improves the mechanical strength and oil-water separation efficiency of the membrane material, achieves excellent hydrophobic properties, and meets the increasingly demanding requirements for oil-water separation.
Smart Images

Figure CN118079666B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of oil-water separation membrane technology, and in particular to a method for preparing a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation. Background Technology
[0002] Traditional oil-water separation methods include biological treatment, coagulation, flotation, and adsorption. However, these methods suffer from low separation efficiency, high energy consumption, complex processes, and the potential for generating secondary pollutants. Therefore, developing an effective oil-water separation technology is urgently needed. In recent years, membrane separation has been widely recognized as the optimal technology for separating oil-water mixtures due to its advantages such as simple operation, high separation efficiency, low manufacturing cost, good flexibility, and environmental controllability. Consequently, increasing research is focusing on polymer-based membrane separation technologies.
[0003] Currently, the existing superhydrophobic composite membranes used for oil-water separation not only have low mechanical strength but also low oil-water separation efficiency, making it difficult for their superhydrophobic properties to meet the increasingly demanding requirements for oil-water separation.
[0004] Therefore, a method for preparing PS / PMMA biomimetic superhydrophobic membranes for oil-water separation is proposed. Summary of the Invention
[0005] Therefore, it is necessary to provide a method for preparing a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation, which addresses the problem that the membrane material has low mechanical strength and low oil-water separation efficiency, making it difficult to meet the increasingly demanding requirements for superhydrophobic performance.
[0006] A method for preparing a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation, wherein the specific steps for preparing the PS / PMMA biomimetic superhydrophobic membrane are as follows:
[0007] (1) Dissolve polystyrene, polymethyl methacrylate and sodium dodecyl sulfate (a pore-forming agent) in tetrahydrofuran and stir until homogeneous to form a stable PS / PMMA mixed solution.
[0008] (2) Immerse the PI membrane in an inorganic acid solution, then add an aniline monomer solution and ammonium persulfate to react and obtain a PI / PANI composite membrane. Remove impurities and dry.
[0009] (3) Carbon nanotubes were pretreated with silane coupling agent and then added to tetrahydrofuran to prepare carbon nanotube dispersion.
[0010] (4) Add the carbon nanotube dispersion obtained in step (3) to the PS / PMMA mixed solution obtained in step (1), disperse it evenly by ultrasonication, then add a poor solvent to promote the separation of the solution phase, and then quickly add it to the substrate. After the film is formed, wash it with water to remove the pore-forming agent and obtain a PS / PMMA biomimetic porous film with a rough surface and uniformly dispersed carbon nanotubes.
[0011] (5) Imprint the biomimetic porous membrane obtained in step (4) onto the PI / PANI composite membrane obtained in step (2), dry and cure to obtain the biomimetic PI / PANI composite membrane.
[0012] (6) The biomimetic PI / PANI composite membrane obtained in step (5) is immersed in PMMA-b-PDMS-b-PS superhydrophobic compound solution to modify the surface of the biomimetic PI / PANI composite membrane with fluorine-containing groups, thereby further improving the hydrophobic properties. The membrane is then removed and subjected to heat treatment to obtain a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation.
[0013] In one embodiment, the PS / PMMA mixed solution in step (1) contains 15-20 parts by weight of polystyrene, 15-20 parts by weight of polymethyl methacrylate, 5-8 parts by weight of sodium dodecyl sulfate as a pore-forming agent, and 52-65 parts by weight of tetrahydrofuran.
[0014] In one embodiment, the amount of ammonium persulfate added in step (2) is 0.0025 to 0.01 mol / L; and the reaction temperature is -8°C to 10°C.
[0015] In one embodiment, the silane coupling agent in step (3) is one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and γ-mercaptopropyltrimethoxysilane; in the carbon nanotube dispersion, there are 2 to 4 parts by weight of silane coupling agent, 5 to 20 parts by weight of carbon nanotubes, and 76 to 93 parts by weight of tetrahydrofuran.
[0016] In one embodiment, the weight parts of each component in step (4) are:
[0017] 40-70 parts by weight of PS / PMMA mixed solution, 10-20 parts by weight of carbon nanotube dispersion, and 20-40 parts by weight of unsuitable solvent; wherein the unsuitable solvent is at least one of ethanol, propanol, n-butanol, sec-butanol, and isopentyl glycol.
[0018] In one embodiment, the substrate in step (4) is one of a ceramic sheet, a quartz sheet, or a glass slide.
[0019] In one embodiment, the PMMA-b-PDMS-b-PS superhydrophobic compound of step (6) is a copolymer of styrene monomer, methyl methacrylate monomer and polydimethylsiloxane.
[0020] In one embodiment, the preparation method of the PMMA-b-PDMS-b-PS superhydrophobic compound specifically includes the following steps:
[0021] S1. Preparation of polydimethylsiloxane: alkoxysilane monomers are hydrolyzed and condensed to obtain polydimethylsiloxane;
[0022] S2, Polydimethylsiloxane end-capping: Add a silane coupling agent to polydimethylsiloxane, stir and mix evenly, add sodium hydroxide and react to obtain amino-double-end-capped polydimethylsiloxane.
[0023] S3. Preparation of initiator: Add azo initiator and DPTS to amino-double-terminated polydimethylsiloxane, then add dichloromethane and DMF, stir and mix evenly to obtain a mixture; add DCC solution to the mixture and stir to react to obtain the initiator;
[0024] S4. Add styrene monomer and methyl methacrylate monomer to the initiator to obtain PMMA-b-PDMS-b-PS superhydrophobic compound.
[0025] In one embodiment, the PMMA-b-PDMS-b-PS superhydrophobic compound has a molecular weight of 2000-10000, the PDMS has a molecular weight of 12000-50000, and the PS has a molecular weight of 5000-300000.
[0026] In one embodiment, the immersion time in step (6) is 3 to 5 hours and the temperature is room temperature.
[0027] The above-mentioned method for preparing a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation utilizes a PI membrane as the substrate material. A biomimetic porous membrane is imprinted on the PI membrane to form a biomimetic PI / PANI composite membrane. A PMMA-b-PDMS-b-PS superhydrophobic compound is then attached to the surface of the biomimetic PI / PANI composite membrane to obtain a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation. Furthermore, a poor solvent is used for phase separation, causing the molecular chains of PS and PMMA to coil into random coils. Finally, a rough structure is formed in which small coils adhere to large coils. This biomimetic structure endows the PS / PMMA membrane with excellent hydrophobic properties. This invention utilizes a PI membrane as the substrate material, which can enhance the mechanical strength of the membrane material while improving the oil-water separation efficiency when combined with a biomimetic porous membrane.
[0028] By adding carbon nanotubes to the composite membrane, the mechanical strength and oil-water separation efficiency of the composite membrane are improved. Furthermore, the biomimetic PI / PANI composite membrane is impregnated with a PMMA-b-PDMS-b-PS superhydrophobic compound solution, which can further improve the hydrophobic properties of the biomimetic PI / PANI composite membrane while ensuring the mechanical strength of the membrane material. Attached Figure Description
[0029] To more clearly illustrate the technical solutions in this invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0030] Figure 1 This is a schematic diagram of the preparation process of the present invention. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0032] It should be noted that when a component is referred to as being "fixed to" or "set on" another component, it can be directly on the other component or there may be an intermediate component. When a component is considered to be "connected to" another component, it can be directly connected to the other component or there may be an intermediate component present. The terms "vertical," "horizontal," "upper," "lower," "left," "right," and similar expressions used in this specification are for illustrative purposes only and do not represent the only possible implementation.
[0033] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0034] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature and the second feature are in indirect contact through an intermediate medium. Furthermore, "above," "over," and "on top" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.
[0035] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used in this specification includes any and all combinations of one or more of the associated listed items.
[0036] Example 1
[0037] The following is combined with Figure 1 The present invention describes a method for preparing a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation. The specific steps for preparing the PS / PMMA biomimetic superhydrophobic membrane are as follows:
[0038] (1) Dissolve polystyrene, polymethyl methacrylate and sodium dodecyl sulfate (a pore-forming agent) in tetrahydrofuran and stir until homogeneous to form a stable PS / PMMA mixed solution.
[0039] (2) Immerse the PI membrane in an inorganic acid solution, then add an aniline monomer solution and ammonium persulfate to react and obtain a PI / PANI composite membrane. Remove impurities and dry.
[0040] (3) Carbon nanotubes were pretreated with silane coupling agent and then added to tetrahydrofuran to prepare carbon nanotube dispersion.
[0041] (4) Add the carbon nanotube dispersion obtained in step (3) to the PS / PMMA mixed solution obtained in step (1), disperse it evenly by ultrasonication, then add a poor solvent to promote the separation of the solution phase, and then quickly add it to the substrate. After the film is formed, wash it with water to remove the pore-forming agent and obtain a PS / PMMA biomimetic porous film with a rough surface and uniformly dispersed carbon nanotubes.
[0042] (5) Imprint the biomimetic porous membrane obtained in step (4) onto the PI / PANI composite membrane obtained in step (2), dry and cure to obtain the biomimetic PI / PANI composite membrane.
[0043] (6) The biomimetic PI / PANI composite membrane obtained in step (5) is immersed in PMMA-b-PDMS-b-PS superhydrophobic compound solution to modify the surface of the biomimetic PI / PANI composite membrane with fluorine-containing groups, thereby further improving the hydrophobic properties. The membrane is then removed and subjected to heat treatment to obtain a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation.
[0044] In this embodiment, the PS / PMMA mixed solution in step (1) contains 15 parts by weight of polystyrene, 15 parts by weight of polymethyl methacrylate, 5 parts by weight of sodium dodecyl sulfate (a pore-forming agent), and 52 parts by weight of tetrahydrofuran.
[0045] In this embodiment, the amount of ammonium persulfate added in step (2) is 0.0025 mol / L; the reaction temperature is -8℃.
[0046] In this embodiment, the silane coupling agent in step (3) is γ-aminopropyltriethoxysilane; in the carbon nanotube dispersion, there are 2 parts by weight of silane coupling agent, 5 parts by weight of carbon nanotubes, and 76 parts by weight of tetrahydrofuran.
[0047] In this embodiment, the weight parts of each component in step (4) are:
[0048] 40 parts by weight of PS / PMMA mixed solution, 10 parts by weight of carbon nanotube dispersion, and 20 parts by weight of unsuitable solvent; the unsuitable solvent is ethanol.
[0049] In this embodiment, the substrate in step (4) is a ceramic sheet.
[0050] In this embodiment, the PMMA-b-PDMS-b-PS superhydrophobic compound in step (6) is a copolymer of styrene monomer, methyl methacrylate monomer and polydimethylsiloxane.
[0051] In this embodiment, the preparation method of the PMMA-b-PDMS-b-PS superhydrophobic compound specifically includes the following steps:
[0052] S1. Preparation of polydimethylsiloxane: alkoxysilane monomers are hydrolyzed and condensed to obtain polydimethylsiloxane;
[0053] S2, Polydimethylsiloxane end-capping: Add a silane coupling agent to polydimethylsiloxane, stir and mix evenly, add sodium hydroxide and react to obtain amino-double-end-capped polydimethylsiloxane.
[0054] S3. Preparation of initiator: Add azo initiator and DPTS to amino-double-terminated polydimethylsiloxane, then add dichloromethane and DMF, stir and mix evenly to obtain a mixture; add DCC solution to the mixture and stir to react to obtain the initiator;
[0055] S4. Add styrene monomer and methyl methacrylate monomer to the initiator to obtain PMMA-b-PDMS-b-PS superhydrophobic compound.
[0056] In this embodiment, the molecular weight of PMMA in the PMMA-b-PDMS-b-PS superhydrophobic compound is 2000, the molecular weight of PDMS is 12000, and the molecular weight of PS is 5000.
[0057] In this embodiment, the immersion time in step (6) is 3 hours and the temperature is room temperature.
[0058] Example 2
[0059] Combination Figure 1 The present invention describes a method for preparing a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation. The specific steps for preparing the PS / PMMA biomimetic superhydrophobic membrane are as follows:
[0060] (1) Dissolve polystyrene, polymethyl methacrylate and sodium dodecyl sulfate (a pore-forming agent) in tetrahydrofuran and stir until homogeneous to form a stable PS / PMMA mixed solution.
[0061] (2) Immerse the PI membrane in an inorganic acid solution, then add an aniline monomer solution and ammonium persulfate to react and obtain a PI / PANI composite membrane. Remove impurities and dry.
[0062] (3) Carbon nanotubes were pretreated with silane coupling agent and then added to tetrahydrofuran to prepare carbon nanotube dispersion.
[0063] (4) Add the carbon nanotube dispersion obtained in step (3) to the PS / PMMA mixed solution obtained in step (1), disperse it evenly by ultrasonication, then add a poor solvent to promote the separation of the solution phase, and then quickly add it to the substrate. After the film is formed, wash it with water to remove the pore-forming agent and obtain a PS / PMMA biomimetic porous film with a rough surface and uniformly dispersed carbon nanotubes.
[0064] (5) Imprint the biomimetic porous membrane obtained in step (4) onto the PI / PANI composite membrane obtained in step (2), dry and cure to obtain the biomimetic PI / PANI composite membrane.
[0065] (6) The biomimetic PI / PANI composite membrane obtained in step (5) is immersed in PMMA-b-PDMS-b-PS superhydrophobic compound solution to modify the surface of the biomimetic PI / PANI composite membrane with fluorine-containing groups, thereby further improving the hydrophobic properties. The membrane is then removed and subjected to heat treatment to obtain a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation.
[0066] In this embodiment, the PS / PMMA mixed solution in step (1) contains 20 parts by weight of polystyrene, 20 parts by weight of polymethyl methacrylate, 8 parts by weight of sodium dodecyl sulfate (a pore-forming agent), and 65 parts by weight of tetrahydrofuran.
[0067] In this embodiment, the amount of ammonium persulfate added in step (2) is 0.01 mol / L; the reaction temperature is 10℃.
[0068] In this embodiment, the silane coupling agent in step (3) is γ-mercaptopropyltrimethoxysilane; in the carbon nanotube dispersion, there are 4 parts by weight of silane coupling agent, 20 parts by weight of carbon nanotubes, and 93 parts by weight of tetrahydrofuran.
[0069] In this embodiment, the weight parts of each component in step (4) are:
[0070] 70 parts by weight of PS / PMMA mixed solution, 20 parts by weight of carbon nanotube dispersion, and 40 parts by weight of unsuitable solvent; the unsuitable solvent is sec-butanol.
[0071] In this embodiment, the substrate in step (4) is a glass slide.
[0072] In this embodiment, the PMMA-b-PDMS-b-PS superhydrophobic compound in step (6) is a copolymer of styrene monomer, methyl methacrylate monomer and polydimethylsiloxane.
[0073] In this embodiment, the preparation method of the PMMA-b-PDMS-b-PS superhydrophobic compound specifically includes the following steps:
[0074] S1. Preparation of polydimethylsiloxane: alkoxysilane monomers are hydrolyzed and condensed to obtain polydimethylsiloxane;
[0075] S2, Polydimethylsiloxane end-capping: Add a silane coupling agent to polydimethylsiloxane, stir and mix evenly, add sodium hydroxide and react to obtain amino-double-end-capped polydimethylsiloxane.
[0076] S3. Preparation of initiator: Add azo initiator and DPTS to amino-double-terminated polydimethylsiloxane, then add dichloromethane and DMF, stir and mix evenly to obtain a mixture; add DCC solution to the mixture and stir to react to obtain the initiator;
[0077] S4. Add styrene monomer and methyl methacrylate monomer to the initiator to obtain PMMA-b-PDMS-b-PS superhydrophobic compound.
[0078] In this embodiment, the molecular weight of PMMA in the PMMA-b-PDMS-b-PS superhydrophobic compound is 10,000, the molecular weight of PDMS is 50,000, and the molecular weight of PS is 300,000.
[0079] In this embodiment, the immersion time in step (6) is 5 hours and the temperature is room temperature.
[0080] Working principle: Polystyrene, polymethyl methacrylate, and sodium dodecyl sulfate (a pore-forming agent) are dissolved in tetrahydrofuran and stirred evenly to form a stable PS / PMMA mixed solution; the PI membrane is immersed in an inorganic acid solution, then an aniline monomer solution is added, and ammonium persulfate is added to react and obtain a PI / PANI composite membrane, which is then cleaned and dried; carbon nanotubes are pretreated with a silane coupling agent and then added to tetrahydrofuran to obtain a carbon nanotube dispersion; the carbon nanotube dispersion obtained in step (3) is added to the PS / PMMA mixed solution obtained in step (1), and ultrasonically dispersed evenly, then a poor solvent is added dropwise to promote phase separation, and then the solution is quickly dispersed. The film is dropped onto a substrate, and after film formation, the pore-forming agent is washed away with water to obtain a PS / PMMA biomimetic porous membrane with a rough surface and uniformly dispersed carbon nanotubes. The biomimetic porous membrane obtained in step (4) is imprinted onto the PI / PANI composite membrane obtained in step (2), dried, and cured to obtain a biomimetic PI / PANI composite membrane. The biomimetic PI / PANI composite membrane obtained in step (5) is immersed in a PMMA-b-PDMS-b-PS superhydrophobic compound solution to modify the surface of the biomimetic PI / PANI composite membrane with fluorine-containing groups, further improving the hydrophobic properties. The membrane is then taken out and subjected to heat treatment to obtain a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation.
[0081] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0082] The above-described embodiments are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the appended claims.
Claims
1. A method for preparing a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation, characterized in that, The specific steps for preparing the PS / PMMA biomimetic superhydrophobic membrane are as follows: (1) Dissolve polystyrene, polymethyl methacrylate and sodium dodecyl sulfate (a pore-forming agent) in tetrahydrofuran and stir until homogeneous to form a stable PS / PMMA mixed solution. (2) Immerse the PI membrane in an inorganic acid solution, then add an aniline monomer solution and ammonium persulfate to react and obtain a PI / PANI composite membrane. Remove impurities and dry. (3) Carbon nanotubes were pretreated with silane coupling agent and then added to tetrahydrofuran to prepare carbon nanotube dispersion. (4) Add the carbon nanotube dispersion obtained in step (3) to the PS / PMMA mixed solution obtained in step (1), disperse it evenly by ultrasonication, then add a poor solvent to promote the separation of the solution phase, and then quickly add it to the substrate. After the film is formed, wash it with water to remove the pore-forming agent and obtain a PS / PMMA biomimetic porous film with a rough surface and uniformly dispersed carbon nanotubes. (5) Imprint the biomimetic porous membrane obtained in step (4) onto the PI / PANI composite membrane obtained in step (2), dry and cure to obtain the biomimetic PI / PANI composite membrane. (6) The biomimetic PI / PANI composite membrane obtained in step (5) is immersed in PMMA-b-PDMS-b-PS superhydrophobic compound solution to modify the surface of the biomimetic PI / PANI composite membrane with fluorine-containing groups to further improve the hydrophobic performance. The membrane is then taken out and subjected to heat treatment to obtain a PS / PMMA biomimetic superhydrophobic membrane for oil-water separation. The PMMA-b-PDMS-b-PS superhydrophobic compound in step (6) is a copolymer of styrene monomer, methyl methacrylate monomer and polydimethylsiloxane. The preparation method of the PMMA-b-PDMS-b-PS superhydrophobic compound specifically includes the following steps: S1. Preparation of polydimethylsiloxane: alkoxysilane monomers are hydrolyzed and condensed to obtain polydimethylsiloxane; S2, Polydimethylsiloxane end-capping: Add a silane coupling agent to polydimethylsiloxane, stir and mix evenly, add sodium hydroxide and react to obtain amino-double-end-capped polydimethylsiloxane. S3. Preparation of initiator: Add azo initiator and DPTS to amino-double-terminated polydimethylsiloxane, then add dichloromethane and DMF, stir and mix evenly to obtain a mixture; add DCC solution to the mixture and stir to react to obtain the initiator; S4. Add styrene monomer and methyl methacrylate monomer to the initiator to obtain PMMA-b-PDMS-b-PS superhydrophobic compound.
2. The method for preparing the PS / PMMA biomimetic superhydrophobic membrane for oil-water separation according to claim 1, characterized in that, In the PS / PMMA mixed solution of step (1), there are 15-20 parts by weight of polystyrene, 15-20 parts by weight of polymethyl methacrylate, 5-8 parts by weight of sodium dodecyl sulfate (a pore-forming agent), and 52-65 parts by weight of tetrahydrofuran.
3. The method for preparing the PS / PMMA biomimetic superhydrophobic membrane for oil-water separation according to claim 1, characterized in that, The amount of ammonium persulfate added in step (2) is 0.0025 to 0.01 mol / L; the reaction temperature is -8℃ to 10℃.
4. The method for preparing the PS / PMMA biomimetic superhydrophobic membrane for oil-water separation according to claim 1, characterized in that, The silane coupling agent in step (3) is one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and γ-mercaptopropyltrimethoxysilane; in the carbon nanotube dispersion, there are 2-4 parts by weight of silane coupling agent, 5-20 parts by weight of carbon nanotubes, and 76-93 parts by weight of tetrahydrofuran.
5. The method for preparing the PS / PMMA biomimetic superhydrophobic membrane for oil-water separation according to claim 1, characterized in that, The weight parts of each component in step (4) are as follows: 40-70 parts by weight of PS / PMMA mixed solution, 10-20 parts by weight of carbon nanotube dispersion, and 20-40 parts by weight of unsuitable solvent; wherein the unsuitable solvent is at least one of ethanol, propanol, n-butanol, sec-butanol, and isopentyl glycol.
6. The method for preparing the PS / PMMA biomimetic superhydrophobic membrane for oil-water separation according to claim 1, characterized in that, The substrate in step (4) is one of ceramic sheet, quartz sheet, or glass slide.
7. The method for preparing the PS / PMMA biomimetic superhydrophobic membrane for oil-water separation according to claim 1, characterized in that, In the PMMA-b-PDMS-b-PS superhydrophobic compound, the molecular weight of PMMA is 2000-10000, the molecular weight of PDMS is 12000-50000, and the molecular weight of PS is 5000-300000.
8. The method for preparing the PS / PMMA biomimetic superhydrophobic membrane for oil-water separation according to claim 1, characterized in that, The soaking time in step (6) is 3 to 5 hours, and the temperature is room temperature.
Citation Information
Patent Citations
Preparation method of PS / PMMA bionic super-hydrophobic membrane for oil-water separation
CN109126205A