Rh-based catalyst, method for preparing the same, and use thereof

By preparing Rh@Al₂O₃ catalyst, the problems of difficult separation of homogeneous catalysts and harsh reaction conditions were solved, and a highly efficient heterogeneous catalyst was provided, which improved the ethanol aldehyde formation rate and selectivity of the formaldehyde hydroformylation reaction and is suitable for industrial applications.

CN118079902BActive Publication Date: 2026-11-24TIANJIN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410206177.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2026-11-24
Estimated Expiration
2044-02-26

AI Technical Summary

Technical Problem

In the existing technology, the catalysts for the formaldehyde hydroformylation reaction are mainly concentrated in homogeneous systems, which have problems such as difficult separation and harsh reaction conditions. There is a lack of research on efficient heterogeneous catalysts.

Method used

The Rh@Al₂O₃ catalyst is prepared by forming a gel with rhodium salt and aluminum nitrate under the promotion of ethylene oxide, followed by calcination and reduction to obtain a heterogeneous catalyst. The active center is Rh and the support is Al₂O₃. The preparation process is simple and reliable and suitable for modular production.

Benefits of technology

It achieves a highly active and selective formaldehyde hydroformylation reaction, significantly improving the formation rate and selectivity of ethanolaldehyde, making it suitable for industrial applications and filling the gap in heterogeneous catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118079902B_ABST
    Figure CN118079902B_ABST
Patent Text Reader

Abstract

This invention discloses an Rh-based catalyst, its preparation method, and its application. The Rh-based catalyst is an Rh@Al2O3 catalyst, with Rh as the active center and Al2O3 as the support. The active center Rh exists in one or more forms, including Rh single atoms, Rh clusters formed by 2-3 Rh single atoms, or Rh nanoparticles formed by Rh clusters. Based on the total weight of the catalyst, the Rh content is 0.16-0.45 wt%. The 0.32% Rh@Al2O3-400 catalyst with an Rh content of 0.32 wt% is beneficial for the activity and selectivity of glycoaldehyde formation. Under the conditions of a reaction pressure of 8 MPa, a reaction temperature of 110 °C, and a phosphine-rhodium ratio of 6, the GA selectivity is 64.9%, and the TOF can reach 402 h⁻¹. ‑1 Compared with the current formaldehyde hydroformylation catalytic system, this invention fills the gap in efficient heterogeneous catalysts, possesses high economic value and market prospects, and is suitable for industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalysts, and more particularly to an Rh-based catalyst, its preparation method and application, specifically an Rh@Al2O3 catalyst and its preparation and application. Background Technology

[0002] Ethylene glycol is an important bulk chemical, mainly used in the production of polyester fibers, packaging resins, and antifreeze. Depending on the raw materials, ethylene glycol production can be divided into oil-based and coal-based routes. The oil-based route uses ethylene as a raw material, produced through ethylene oxide rehydration, and is the globally adopted production process. The industrially used coal-based route uses syngas as a raw material, methyl nitrite as a reaction medium, and carbonylation and hydrogenation to produce ethylene glycol. Although this route can achieve ethylene glycol yields of over 95%, it generates a large amount of NO in the process. x Pollution and high overall energy consumption are inherent problems in ethylene glycol production. The one-step synthesis of ethylene glycol from syngas theoretically offers a simpler process that can significantly reduce costs. Furthermore, as an atom-economic process, it maximizes the utilization of every atom in the reactants, making it extremely economical. The entire route comprises three parts: syngas to formaldehyde, formaldehyde hydroformylation to glycolaldehyde, and glycolaldehyde hydrogenation to ethylene glycol. The formaldehyde hydroformylation step significantly impacts the activity and selectivity of the entire reaction. Developing a highly active, selective, and stable formaldehyde hydroformylation catalyst could greatly improve ethylene glycol production technology, representing a revolutionary advancement.

[0003] Formaldehyde hydroformylation is primarily a homogeneous system, with commonly used metal centers including Rh, Co, and Ru. Early studies mainly focused on Co-based catalysts. Yukawa et al., using Co2(CO)8 as a precursor, found that Co's ability to insert CO into form C-C bonds was weak, and the reaction typically required extremely high temperatures (200 °C) and pressures (20 MPa) (US 3920753). In 1977, Monsanto disclosed a homogeneous formaldehyde hydroformylation catalyst using metal Rh as the active component in combination with trialkylphosphine ligands, which significantly improved the yield of ethanolaldehyde. Furthermore, compared to the Co system, the required reaction conditions were milder (EP 0002908). Up to this point, the vast majority of research was based on the Rh system. During this period, Marchionna et al. also investigated the activity of Ru-based catalysts, but the results were not ideal (J. Mol. Catal. 1989, 57, 2, 221-235). In general, the catalyst activities currently used for the hydroformylation of formaldehyde are roughly as follows: Rh >> Co > Ru, and the majority of studies are on the Rh system.

[0004] In homogeneous catalysis, the catalyst is dispersed at the molecular level in the liquid phase, allowing for sufficient contact between the substrate and the active site, often resulting in extremely high catalytic performance. However, homogeneous complex catalysts are often highly sensitive to temperature, pressure, and moisture, and are particularly difficult to separate from the product without damaging the ligands. The hydroformylation of formaldehyde typically employs a noble metal rhodium-based catalytic system with a large number of ligands. The subsequent separation in homogeneous systems presents a significant challenge. Heterogeneous catalysis, on the other hand, facilitates separation because the catalyst, reactants, and products exist in different phases. Furthermore, existing literature on heterogeneous systems for the hydroformylation of formaldehyde is scarce; therefore, designing and developing heterogeneous catalysts is an important supplement and improvement to this field. Based on this, this invention is proposed. Summary of the Invention

[0005] The present invention aims to provide a heterogeneous Rh@Al2O3 catalyst for the hydroformylation reaction of formaldehyde, which has high activity and high selectivity.

[0006] Another objective of this invention is to provide a preparation method for an Rh-based catalyst for the hydroformylation reaction of formaldehyde, which is characterized by its simplicity and high reliability.

[0007] To achieve the above objectives, this invention provides a Rh@Al2O3 catalyst for the hydroformylation of formaldehyde, its preparation, and its application. The active center is Rh, and the support is Al2O3. Based on the total weight of the catalyst, the Rh content is 0.16~0.45 wt%. The catalyst preparation process involves forming a gel with a certain amount of rhodium salt and aluminum nitrate under the promotion of ethylene oxide, followed by calcination and reduction to obtain the Rh@Al2O3 catalyst. Utilizing the unique geometric structure and electronic effects of the active center and support, this catalyst achieves extremely high reaction performance, filling the gap in heterogeneous catalysis research in the field of formaldehyde hydroformylation.

[0008] To achieve the objectives of this invention, the specific technical solution is as follows:

[0009] The first aspect of the present invention provides an Rh-based catalyst, wherein the Rh-based catalyst is an Rh@Al2O3 catalyst, the active center of which is Rh and the support is Al2O3, and the Rh content is 0.16~0.45 wt% based on the total weight of the catalyst.

[0010] A second aspect of the present invention provides a method for preparing the Rh@Al2O3 catalyst described in the first aspect of the present invention, comprising the following steps:

[0011] 1) Preparation of raw material solution: Dissolve the rhodium source sample and the aluminum source sample in a mixture of ethanol and water in a certain proportion, heat and stir until completely dissolved to obtain the raw material solution;

[0012] 2) Gel formation: Add propylene oxide dropwise to the raw material solution obtained in step 1) until gel formation is achieved, and then wash with deionized water and ethanol to obtain the colloid.

[0013] 3) Aging: Seal the colloid obtained in step 2) with anhydrous ethanol, age it for a period of time, and then place it in a vacuum oven to dry and remove excess liquid to obtain a mixture;

[0014] 4) Calcination: The mixture obtained in step 3) is calcined at high temperature in a muffle furnace to obtain a particulate catalyst precursor;

[0015] 5) Activation: Grind the particulate catalyst precursor obtained in step 4) until there is no obvious particle feel to obtain catalyst powder, and then activate the catalyst powder under a reducing atmosphere to obtain Rh@Al2O3 catalyst.

[0016] Preferably, in step 1), the rhodium source is any one of rhodium chloride and rhodium acetylacetonate, and the aluminum source is any one of aluminum chloride and aluminum nitrate; the volume ratio of ethanol to water is 3-1; the stirring temperature is 70-90 °C; and the stirring time is 0.5-2 h. More preferably, rhodium acetylacetonate and aluminum nitrate are dissolved in a mixture of ethanol and water (volume ratio of ethanol to water 2.25), and stirred in an oil bath at 80 °C for 1 h to obtain an orange-yellow raw material solution.

[0017] Preferably, in step 2), the volume ratio of propylene oxide to the raw material liquid is 0.7 to 1. More preferably, the volume ratio of propylene oxide to the raw material liquid is 0.82.

[0018] Preferably, in step 3), the aging time is 1~24 h, the oven drying temperature is 40~70 ℃, and the drying time is 1~12 h. More preferably, the aging time is 24 h, the oven drying temperature is 45 ℃, and the drying time is 8 h.

[0019] Preferably, in step 4), the calcination conditions are to raise the temperature from room temperature to 300-600°C at a heating rate of 1-15°C / min and maintain it for 2-24 h. More preferably, the sample is heated in a muffle furnace from room temperature to 300-600°C at a heating rate of 5°C / min and maintained for 8 h.

[0020] Preferably, in step 5), the reducing gas is hydrogen with a purity greater than 99.9%, or the reducing gas is a hydrogen-containing mixture in which hydrogen accounts for 10-100% of the volume, and the other gases besides hydrogen are nitrogen or helium; the flow rate of the reducing gas is 10-25 mL / min, the reduction temperature is 150-300 °C, the temperature program is from room temperature to the target reduction temperature at a rate of 1-15 °C / min, the pressure is atmospheric pressure, and the reduction time is 1-4 h. More preferably, the flow rate of the reducing gas is 20 mL / min, the reduction temperature is 200 °C, the temperature program is from room temperature to the target reduction temperature at a rate of 5 °C / min, the pressure is atmospheric pressure, and the reduction time is 90 min.

[0021] A third aspect of the present invention provides an application of the Rh@Al2O3 catalyst described in the first aspect of the present invention, wherein the Rh@Al2O3 catalyst is used as a heterogeneous catalyst in the hydroformylation reaction of formaldehyde.

[0022] Preferably, the Rh@Al2O3 catalyst is used for the hydroformylation reaction of formaldehyde in a batch reactor, and the reaction conditions are as follows: the reaction raw material is a mixture of CO and H2 gas with a molar ratio of 1 to 3, the reaction temperature is 90 to 120 °C, the pressure is 6 to 9 MPa, and the ratio of triphenylphosphine ligand to active center is 3 to 24.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention successfully prepared Rh@Al2O3 catalyst, wherein the active center Rh exists in one or more forms, such as Rh single atom, Rh atom cluster formed by Rh single atom, or Rh nanoparticle formed by Rh atom cluster, and the Rh content is 0.16~0.45 wt% based on the total weight of the catalyst.

[0025] 2. The present invention obtains Rh@Al2O3 catalyst by forming a gel with rhodium salt and aluminum nitrate under the promotion of ethylene oxide, followed by calcination and reduction. The preparation method is simple and reliable, the preparation process is easy to operate, and it is suitable for modular production.

[0026] 3. The Rh@Al2O3 catalyst provided by this invention uses Al2O3 support, which can form a strong interaction force with Rh, effectively inhibiting sintering and agglomeration, maintaining single-atom and small cluster states, and significantly improving the yield and selectivity of the main product glycoaldehyde GA.

[0027] 4. In this invention, the Rh content is 0.32 wt% (0.32% Rh@Al2O3-400 catalyst), which is beneficial to the activity and selectivity of glycolaldehyde formation. Under the conditions of reaction pressure of 8 MPa, reaction temperature of 110℃, and phosphine-rhodium ratio of 6, the GA selectivity is 64.9%, and the calculated TOF can reach 402 h. -1 .

[0028] 5. Compared with the current formaldehyde hydroformylation catalytic system, this invention fills the gap in efficient heterogeneous catalysts, has high economic value and market prospects, and is suitable for industrial applications. Attached Figure Description

[0029] Figure 1 CO-IR spectra of Rh@Al2O3 catalysts with different Rh contents;

[0030] Figure 2 Aberration-corrected electron microscopy images of Rh@Al2O3 catalysts with different Rh contents are shown, where (a) represents 0.16% Rh@Al2O3, (b) represents 0.32% Rh@Al2O3, and (c) represents 0.45% Rh@Al2O3.

[0031] Figure 3 CO-IR spectra of Rh@Al2O3 catalysts at different calcination temperatures;

[0032] Figure 4 Transmission electron microscopy (TEM) images of Rh@Al2O3 catalysts at different calcination temperatures, where (a) is under calcination at 300℃, (b)(c) is under calcination at 400℃, (d)(e) is under calcination at 500℃, and (f)(g) is under calcination at 600℃.

[0033] Figure 5 The CO-TPD diagrams are for Rh@Al2O3 catalysts at different calcination temperatures. Detailed Implementation

[0034] The present invention will be described below with reference to specific embodiments, but the implementation of the present invention is not limited thereto. Experimental methods not specifically described in the embodiments are generally performed under conventional conditions and conditions described in the manual, or according to the manufacturer's recommendations. Unless otherwise specified, the general equipment, materials, reagents, etc., used are commercially available. The raw materials required in the following embodiments and comparative examples are all commercially available.

[0035] Examples 1-3 illustrate the preparation of Rh@Al2O3 catalysts with different Rh contents:

[0036] Example 1

[0037] Measure 12 mL of deionized water and 27 mL of anhydrous ethanol and mix thoroughly. Weigh 18.76 g of Al(NO3)3·9H2O and 127.82 mg of Rh(CO)2(acac) and dissolve them in the above solution. Stir magnetically at 80 °C for 1 h under normal pressure. After cooling at room temperature for 1 h, add a total of 32 mL of propylene oxide dropwise at a rate of 1 drop per second. After standing at room temperature for about 30 min, the solution forms a gel. Wash the colloid three times with deionized water and then wash it twice with anhydrous ethanol. Seal the colloid with anhydrous ethanol and allow it to age for 24 h. After discarding the sealing solution, place the colloid in a vacuum oven to dry at 45 °C for 8 h. Place the dried sample in a muffle furnace and heat it from room temperature to 400 °C at a rate of 5 °C / min, and maintain the temperature for 8 h. Subsequently, the material was reduced and activated at 200 °C and a hydrogen atmosphere at a flow rate of 20 mL / min for 90 min to obtain 0.45% Rh@Al2O3-400.

[0038] Example 2

[0039] Except for the amount of Rh(CO)2(acac) being 63.91 mg, the preparation method was exactly the same as in Example 1, yielding 0.32% Rh@Al2O3-400.

[0040] Example 3

[0041] Except for the amount of Rh(CO)2(acac) being 32.25 mg, the preparation method was exactly the same as in Example 1, yielding 0.16% Rh@Al2O3-400.

[0042] Examples 4-6 illustrate the preparation of Rh@Al2O3 catalysts at different calcination temperatures:

[0043] Example 4

[0044] Measure 12 mL of deionized water and 27 mL of anhydrous ethanol and mix thoroughly. Weigh 18.76 g of Al(NO3)3·9H2O and 63.91 mg of Rh(CO)2(acac) and dissolve them in the above solution. Stir magnetically at 80 °C for 1 h under normal pressure. After cooling at room temperature for 1 h, add a total of 32 mL of propylene oxide dropwise at a rate of 1 drop per second. After standing at room temperature for about 30 min, the solution forms a gel. Wash the colloid three times with deionized water and then wash it twice with anhydrous ethanol. Seal the colloid with anhydrous ethanol and allow it to age for 24 h. After discarding the sealing solution, place the colloid in a vacuum oven to dry at 45 °C for 8 h. Place the dried sample in a muffle furnace and heat it from room temperature to 300 °C at a rate of 5 °C / min, and maintain the temperature for 8 h. Subsequently, the material was reduced and activated at 200 °C and a hydrogen atmosphere at a flow rate of 20 mL / min for 90 min to obtain 0.32% Rh@Al2O3-300.

[0045] Example 5

[0046] Except for the calcination temperature of the sample in the muffle furnace being 500 °C, the other preparation methods were exactly the same as in Example 4, yielding 0.32% Rh@Al2O3-500.

[0047] Example 6

[0048] Except for the calcination temperature of the sample in the muffle furnace being 600 °C, the other preparation methods were exactly the same as in Example 4, yielding 0.32% Rh@Al2O3-600.

[0049] Comparative infrared spectra of the CO adsorption of the catalysts obtained in Examples 1-3 are shown in the attached figures. Figure 1 As shown. All three catalysts with varying Rh contents were at 2008 cm⁻¹. -1 With 2083 cm -1 The peak at this position can be attributed to the symmetric and asymmetric vibrational peaks of the dicarbonyl group, commonly found in single-atom Rh catalysts. Example 1 shows a peak at 2042 cm⁻¹. -1 With 1835 cm -1 Additional spectral bands exist, corresponding to the line vibration peak and bridge vibration peak of the carbonyl group, respectively, which are commonly found in nanoparticle catalysts. Aberration-corrected electron microscopy images of the catalysts obtained in Examples 1-3 are attached. Figure 2As shown, in the low-loaded catalyst (Example 3), the vast majority of Rh exists in single-atom form, with a very small amount of small clusters containing 2-3 atoms. With increased catalyst loading (Example 2), although Rh is still predominantly single-atom, the proportion of small clusters begins to increase. In Example 1, in addition to single atoms and small clusters, Rh nanoparticles with a diameter of approximately 1 nm were clearly observed to form. In summary, the form of metal in the catalyst changes significantly with increasing loading, transitioning from single atoms to nanoparticles.

[0050] Comparative infrared spectra of the CO adsorption of the catalysts obtained in Examples 2 and 4-6 are shown in the attached figures. Figure 3 As shown. All catalysts were only at 2008 cm⁻¹. -1 With 2083 cm -1 The peak at the specified location indicates that no agglomeration occurred at the metal center. Transmission electron microscopy (TEM) images of the catalysts obtained in Examples 2 and 4-6 are attached. Figure 4 As shown, with increasing calcination temperature, the crystal form of the support gradually transforms from amorphous to γ-Al₂O₃. The CO-TPD diagrams of the catalysts obtained in Examples 2 and 4-6 are shown in the attached figures. Figure 5 As shown, Example 4 exhibits three CO desorption peaks, located at 274 °C, 340 °C, and 425 °C, respectively. The latter two desorption temperatures are higher than the catalyst calcination temperature (300 °C), possibly due to changes in the support's crystal phase. For the desorption peak near 270 °C, the desorption temperature gradually shifts to lower temperatures with increasing calcination temperature. In summary, changing the catalyst calcination temperature does not affect the morphology of the active centers, but it alters the crystal structure of the support, thereby modulating the interaction force between the metal and the support and weakening the adsorption capacity of the metal centers for reactants.

[0051] The catalysts obtained in Examples 1-6 were used for the hydroformylation of formaldehyde, and their catalytic activities were compared. The procedure was as follows: 0.6 g of paraformaldehyde, 200 mg of catalyst, and 8-63 mg of triphenylphosphine ligand were weighed into a reactor. The reactor was flushed three times with 3 MPa syngas (CO to H2 molar ratio of 1:1) to replace the gas inside. After pressurizing to 10 MPa, stirring was started at 600 rpm and maintained for a period of time to ensure the experimental apparatus was safe and leak-free. After stirring was stopped, the pressure was released to 1 MPa. The temperature was raised to the target temperature (90-120 °C), and the pressure was increased to the target pressure (6-9 MPa). Stirring was started at 600 rpm, and the reaction was started and timed for 1 h.

[0052] After the reaction was complete, heating and stirring were turned off, and the reactor was removed and allowed to cool naturally in air before depressurization. Approximately 0.6 g of internal standard isopropanol was weighed and added to the reaction solution. After thorough stirring, the solution was filtered and subjected to gas chromatography analysis. The instrument was a Shimadzu GC-2014, equipped with a WondaCap FFAP capillary column (30 m × 0.53 mm × 1 μm) and a PorapakT packed column. The detectors included a flame ionization detector (FID) and a thermal conductivity detector (TCD). Formaldehyde was separated using the packed column and quantitatively analyzed by the TCD. The injection port and detector temperatures were maintained at 200 °C. The temperature program first held at 90 °C for 1 min, then increased to 180 °C at a rate of 20 °C / min and held for 1 min. High-purity helium was used as the carrier gas at a flow rate of 35 mL / min. The remaining components in the reaction solution were separated using the capillary column and quantitatively analyzed by the flame ionization detector. The injection port and detector temperatures were maintained at 250 °C. The temperature program first held at 60 °C for 2 min, then increased to 90 °C at a rate of 20 °C / min and held for 1 min, and finally increased to 180 °C at a rate of 20 °C / min and held for 15 min. High-purity helium was used as the carrier gas at a flow rate of 75 mL / min.

[0053] The test results are shown in Appendix 1, Appendix 2, Appendix 3, Appendix 4 and Appendix 5.

[0054] The performance of catalysts with different Rh loadings was compared under the following reaction conditions: reaction pressure 7 MPa, reaction temperature 110 °C, and phosphine-rhodium ratio 6. The results are shown in Table 1. Since CO-IR and aberration-corrected electron microscopy characterization results have shown that the 0.16% and 0.32% loaded catalyst metals are predominantly single-atom, their Time-of-Flight (TOF) was calculated for easier performance comparison. With increasing loading, the selectivity for the main product, ethanolaldehyde, first increased and then remained relatively constant around 57%; while the yield first increased and then decreased and remained constant, reaching its highest point at 0.32%. This may be because in the heterogeneous system, the formation of ethanolaldehyde requires the participation of Rh clusters. When the catalyst metal loading is low, the catalyst contains only a very small amount of Rh clusters, and the formation of methanol as a byproduct is dominant. With increasing loading, the proportion of Rh clusters increases, and the formation of the main product, ethanolaldehyde, becomes dominant. When the loading is further increased, Rh nanoparticles are formed, wasting a large number of active sites, and the yield of ethanolaldehyde decreases, but the selectivity remains unchanged, unaffected by the formation of nanoparticles.

[0055] Table 1. Comparison of formaldehyde hydroformylation performance of Rh@Al2O3 catalysts with different Rh contents

[0056]

[0057] The performance of catalysts calcined at different temperatures was compared. The specific reaction conditions were set as follows: reaction pressure 7 MPa, reaction temperature 110 °C, and phosphine-rhodium ratio 6. The results are shown in Table 2. With increasing calcination temperature, the selectivity of the reaction first increased and then decreased, with the catalyst calcined at 400 °C showing the highest selectivity for ethanolaldehyde. The formation rate of the main ethanolaldehyde product showed a similar trend, with the highest TOF obtained at 400 °C calcination. GA (403 h) -1 The activity of the by-product methanol did not change significantly with increasing calcination temperature, and the TOF remained at 200 h. -1 The adsorption capacity of the catalyst for CO was optimal at 400 °C, based on the characterization results of CO-TPD. At 300 °C, the catalyst exhibited stronger CO adsorption, enhancing the energy barrier of the carbonyl insertion step in the ethanolaldehyde route, thus inhibiting ethanolaldehyde formation while having little effect on methanol. As the calcination temperature increased, the catalyst's CO adsorption weakened, reducing the stability of the carbonyl rhodium phosphine complex in the cycle and consequently decreasing the formation rates of both ethanolaldehyde and methanol.

[0058] Table 2 Comparison of formaldehyde hydroformylation performance of Rh@Al2O3 catalysts at different calcination temperatures

[0059]

[0060] Using the sample from Example 2 as the catalyst, the catalyst performance under different reaction pressure conditions was compared, and the results are shown in Table 3. Overall, the reaction is not sensitive to changes in pressure, and the TOF of ethanolaldehyde remains at 400 h⁻¹. -1 Nearby, the TOF of methanol was at 220 h. -1 Up to 250 h -1 Within the range.

[0061] Table 3. Comparison of formaldehyde hydroformylation performance of Rh@Al2O3 catalysts under different reaction pressures

[0062]

[0063] The catalyst performance under different reaction temperatures was compared, and the results are shown in Table 4. With increasing reaction temperature, the activities of both ethanolaldehyde and methanol significantly improved. The growth rate of ethanolaldehyde gradually slowed down, while the growth rate of methanol was greater. The selectivity of the reaction first increased and then decreased, exhibiting a volcanic pattern. At a temperature of 110 °C, the selectivity for the main ethanolaldehyde production reached its highest level (64.9%), while maintaining a relatively high activity.

[0064] Table 4. Comparison of formaldehyde hydroformylation performance of Rh@Al2O3 catalysts at different reaction temperatures

[0065]

[0066] The catalyst performance under different phosphine ligand concentrations was compared, and the results are shown in Table 5. With increasing ligand concentration, the selectivity of ethanolaldehyde initially remained constant and then slowly decreased. The formation rate of ethanolaldehyde initially increased and then decreased, reaching its highest point at a phosphine-to-rhodium ratio of 6, while the formation rate of methanol increased slowly. This phenomenon may be due to the decomposition of ligands during the reaction. When the phosphine-to-rhodium ratio is low, the ligands in the solution gradually decompose as the reaction proceeds, and the lack of ligands to coordinate with the metal center leads to a decrease in activity. When the phosphine-to-rhodium ratio is too high, excessive ligands coordinate with the metal center, inhibiting the formation of ethanolaldehyde.

[0067] Table 5. Comparison of formaldehyde hydroformylation performance of Rh@Al2O3 catalysts with different phosphine ligand concentrations

[0068]

[0069] Unless otherwise specified, the raw materials and equipment used in this invention are all commonly used in the field; unless otherwise specified, the methods used in this invention are all conventional methods in the field.

[0070] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, alterations, and equivalent transformations made to the above embodiments based on the technical essence of the present invention shall still fall within the protection scope of the present invention.

Claims

1. A Rh-based catalyst, characterized in that, The Rh-based catalyst is an Rh@Al2O3 catalyst, with Rh as the active center and Al2O3 as the support. The active center Rh exists in one or more forms: Rh single atoms, Rh clusters formed by 2-3 Rh single atoms, or Rh nanoparticles formed by Rh clusters. Based on the total weight of the catalyst, the Rh content is 0.16~0.45 wt%. The method for preparing the Rh-based catalyst includes the following steps: 1) Preparation of raw material solution: Dissolve the rhodium source sample and the aluminum source sample in a mixture of ethanol and water in a certain proportion, heat and stir until dissolved to obtain the raw material solution; 2) Gel formation: Add propylene oxide dropwise to the raw material solution obtained in step 1) until gel formation is achieved, and then wash with deionized water and ethanol to obtain the colloid. 3) Aging: Seal the colloid obtained in step 2) with anhydrous ethanol, age it for a period of time, and then dry it to remove excess liquid to obtain a mixture; 4) Calcination: The mixture obtained in step 3) is calcined in a muffle furnace to obtain a particulate catalyst precursor; 5) Activation: The particulate catalyst precursor obtained in step 4) is ground and then activated under a reducing atmosphere to obtain the target Rh@Al2O3 catalyst.

2. The Rh-based catalyst according to claim 1, characterized in that, Based on the total weight of the catalyst, the Rh content is 0.32 wt%, and the active center Rh in the Rh@Al2O3 catalyst exists in two forms: Rh single atoms and Rh atom clusters formed by Rh single atoms.

3. The Rh-based catalyst according to claim 1, characterized in that, In step 1), the rhodium source is any one of rhodium chloride and rhodium acetylacetonate, and the aluminum source is any one of aluminum chloride and aluminum nitrate; the volume ratio of ethanol to water is 3~1; the stirring temperature is 70~90 ℃; and the stirring time is 0.5~2 h.

4. The Rh-based catalyst according to claim 1, characterized in that, In step 2), the volume ratio of propylene oxide to the raw material liquid is 0.7~1.

5. The Rh-based catalyst according to claim 1, characterized in that, In step 3), the aging time is 1~24 h, the drying temperature is 40~70 ℃, and the drying time is 1~12 h.

6. The Rh-based catalyst according to claim 1, characterized in that, In step 4), the calcination conditions are to raise the temperature from room temperature to 300-600 ℃ at a heating rate of 1-15 ℃ / min and maintain it for 2-24 h.

7. The Rh-based catalyst according to claim 1, characterized in that, In step 5), the reducing gas is hydrogen with a purity greater than 99.9%; the flow rate of the reducing gas is 10~25 mL / min, the reduction temperature is 150~300 ℃, the programmed temperature rises from room temperature to the target reduction temperature at a rate of 1~15 ℃ / min, the pressure is atmospheric pressure, and the reduction time is 1~4 h.

8. The application of the Rh-based catalyst according to any one of claims 1-7, characterized in that, The Rh@Al2O3 catalyst described herein is used as a heterogeneous catalyst in the hydroformylation reaction of formaldehyde.

9. The application according to claim 8, characterized in that, The Rh@Al2O3 catalyst is used for the hydroformylation of formaldehyde in a batch reactor. The reaction conditions are as follows: the reaction feedstock is a mixture of CO and H2 gas with a molar ratio of 1 to 3, the reaction temperature is 90 to 120 °C, the pressure is 6 to 9 MPa, and the ratio of triphenylphosphine ligand to active center is 3 to 24.

Citation Information

Patent Citations

  • Hydroformylation of formaldehyde with rhodium catalyst

    EP0002908A1

  • Method of producing glycolaldehyde

    US3920753A

  • Preparation method of ultra-light blocky aluminum oxide aerogel

    CN106395873A

  • Method for regulating existence form of Rh species in rhodium-based catalyst

    CN115382541A