Indium-based catalysts and methods for their preparation

The preparation of indium-based catalysts by water bath heating co-precipitation method solves the problems of low conversion rate and complex preparation of indium-based catalysts in the existing technology, realizes a highly efficient process for the hydrogenation of carbon dioxide to methanol, improves catalytic activity and stability, and is suitable for large-scale production.

CN118079934BActive Publication Date: 2026-11-24EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410175775.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-07
Publication Date
2026-11-24
Estimated Expiration
2044-02-07

AI Technical Summary

Technical Problem

Existing indium-based catalysts have low conversion rates in the process of producing methanol from carbon dioxide hydrogenation, and traditional preparation methods suffer from uneven element distribution and complex preparation processes.

Method used

Indium-based catalysts were prepared by a water bath heating co-precipitation method. By controlling the pH value and stirring speed, uniform indium, cobalt, and zirconium particles were formed. The catalyst was then calcined at 450°C to form a highly active catalyst.

Benefits of technology

It improves the activity and stability of the catalyst, reduces diffusion resistance, is suitable for mass production, avoids the shortcomings of supported catalysts in traditional methods, and improves the efficiency of carbon dioxide to methanol conversion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118079934B_ABST
    Figure CN118079934B_ABST
Patent Text Reader

Abstract

The present application relates to a kind of indium-based catalyst and its preparation method, by indium salt, cobalt salt, zirconium salt, sodium carbonate is added dropwise mixed under certain pH and temperature and stirring is carried out reaction, the solid-liquid separation of synthesis product is carried out, then by washing, drying and calcining, so that the indium-based catalyst is prepared.The indium-based catalyst is used for the reaction of carbon dioxide hydrogenation preparation methanol, and has high catalytic reaction activity and excellent methanol selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an indium-based catalyst and its preparation method, particularly to an indium-based catalyst that can be used for the hydrogenation of carbon dioxide to synthesize methanol and a method for preparing the indium-based catalyst. Background Technology

[0002] Carbon dioxide (CO) 2) Carbon is currently considered a major anthropogenic greenhouse gas, and therefore, it is often used as a substitute for greenhouse gases in various countries' neutralization or net-zero emission targets. Consequently, CO2 emission reduction and control have received considerable attention. Using carbon dioxide as a raw material to produce valuable carbon-containing products offers a cost-effective and environmentally friendly solution for chemical production.

[0003] Methanol is an important intermediate in chemical synthesis and can also be used directly as fuel. The production of methanol via carbon dioxide hydrogenation has significant economic potential and is expected to be produced on a large scale. A class of catalysts based on Cu / ZnO are most commonly used in industrial production. Typically, methanol formation must compete with the reverse water gas (RWGS) reaction, which produces carbon monoxide (CO), the most common and major byproduct in methanol production. Furthermore, compared to methanol formation reactions, the RWGS reaction is more temperature-sensitive and proceeds more readily at higher temperatures; therefore, most catalysts limit reaction temperature and pressure to a range below 250°C and above 7 MPa.

[0004] Indium trioxide (In₂O₃) also exhibits activity in the hydrogenation of CO₂ to methanol. Compared to copper-based catalysts, it has lower activity in the competing reaction RWGS for methanol production, thus avoiding the formation of carbon monoxide. Due to the high selectivity and stability of In₂O₃ at higher temperatures, indium-based catalysts have received widespread attention and research. However, the CO₂ conversion rate catalyzed by pure In₂O₃ remains relatively low.

[0005] Therefore, it is necessary to provide an indium-based catalyst and its preparation method, which can be used to synthesize methanol from carbon dioxide via hydrogenation reaction, in order to solve the problems existing in the prior art. Summary of the Invention

[0006] The main objective of this invention is to provide an indium-based catalyst and its preparation method. The preparation method of the indium-based catalyst is simple, suitable for large-scale production, low in cost, and environmentally friendly. The indium-based catalyst exhibits high catalytic activity and good stability in the catalytic hydrogenation of carbon dioxide to methanol, overcoming the low conversion rate of methanol production from pure In₂O₃.

[0007] To achieve the above objectives, one embodiment of the present invention provides an indium-based catalyst comprising: a metal component comprising indium, cobalt, and zirconium, wherein the molar ratio of indium to the metal component is 0.5 to 0.9, and the molar ratio of cobalt to zirconium is less than 10.

[0008] Another embodiment of the present invention provides a method for preparing an indium-based catalyst, the method comprising the following steps:

[0009] (S1) Prepare a metal salt solution containing at least one metal salt, wherein the metal salt includes indium salt, cobalt salt and zirconium salt, and the concentration of the metal salt solution is 0.25 to 0.55 mol / L;

[0010] (S2) Prepare a sodium carbonate solution and add it dropwise to the metal salt solution to form a reaction solution;

[0011] (S3) Maintain the pH of the reaction solution between 8.5 and 0.3, and carry out the reaction at 55 to 65°C to form a solid product;

[0012] (S4) After cooling at room temperature, remove and wash the solid product; and

[0013] (S5) The solid product is calcined in air at 350 to 550°C to form the above-mentioned indium-based catalyst.

[0014] In one embodiment of the present invention, in step (S1), the indium salt is indium nitrate, the cobalt salt is cobalt nitrate, and the zirconium salt is zirconium nitrate.

[0015] In one embodiment of the present invention, in step (S1), the molar ratio of the indium salt to the metal salt is 0.5 to 0.9.

[0016] In one embodiment of the present invention, in step (S1), the molar ratio of the cobalt salt and the zirconium salt is less than 10.

[0017] In one embodiment of the present invention, in step (S2), the sodium carbonate solution has a concentration of 0.15 to 0.45 mol / L.

[0018] In one embodiment of the present invention, step (S2) further includes stirring the reaction solution at a speed of 250 to 350 rpm for 0.5 to 2 hours.

[0019] In one embodiment of the present invention, in step (S4), the reaction solution is cooled to room temperature and aged for 10 to 14 hours.

[0020] In one embodiment of the invention, step (S4) is followed by drying the solid product at 100 to 120°C for 10 to 14 hours.

[0021] In one embodiment of the present invention, in step (S5), the solid product is calcined for 5 to 7 hours.

[0022] The beneficial effects of this invention are:

[0023] The indium-based catalyst of this invention is prepared by a co-precipitation synthesis strategy using water bath heating. Compared with indium-based catalysts prepared by hydrothermal synthesis and impregnation methods, it has the following substantial features and advancements:

[0024] (1) The unsupported indium-based catalyst prepared by the method of this invention avoids the disadvantages of uneven element distribution and weak intermetallic interaction in the impregnation method. Furthermore, the pH value is controlled by slowly adding the catalyst and stirring to regulate the co-precipitation rate. Therefore, compared with catalysts prepared by ordinary precipitation methods, the indium-based catalyst prepared by this invention has smaller and more uniform particle size, which can improve the mass transfer of the feed gas, reduce diffusion resistance, and enhance catalytic activity. In addition, compared with hydrothermal synthesis methods, the preparation method of this invention is simpler and suitable for mass production.

[0025] (2) This invention investigated the effect of calcination temperature on the reactivity of indium-based catalysts and found that catalysts calcined at 450°C exhibited the best reactivity. This invention also addresses the influence of different alkaline solutions (precipitants) on the reactivity of indium-based catalysts in the hydrogenation of carbon dioxide to methanol, providing a reference for large-scale industrial production. Attached Figure Description

[0026] Figure 1 This is a schematic flowchart of a method for preparing an indium-based catalyst according to an embodiment of the present invention. Detailed Implementation

[0027] To make the above and other objects, features, and advantages of the present invention more apparent and understandable, preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Furthermore, the singular forms “a,” “an,” and “described” used in this invention include plural references unless the context clearly specifies otherwise. Numerical ranges (e.g., 10% to 11% of A) include upper and lower limits unless specifically stated otherwise (i.e., 10% ≤ A ≤ 11%); if a numerical range does not define a lower limit (e.g., less than 0.2% of B, or B below 0.2%), it means that the lower limit may be 0 (i.e., 0% ≤ B ≤ 0.2%). The above terms are used to illustrate and understand the present invention, and not to limit the present invention.

[0028] One embodiment of the present invention provides an indium-based catalyst, which mainly comprises at least one metal component, said metal component including indium, cobalt, and zirconium. The molar ratio of indium to said metal component is 0.5 to 0.9, and may be, for example, 0.5, 0.6, 0.7, 0.8, or 0.9, or any other value between 0.5 and 0.9. The molar ratio of cobalt to said zirconium is less than 10, and may be, for example, 1, 2, 3, 5, 7, 9, or 10, or any other integer or non-integer value between 0 and 10.

[0029] Another embodiment of the present invention provides a method for preparing an indium-based catalyst, which mainly includes the following steps: (S1) preparing a metal salt solution with a concentration of 0.25 to 0.55 mol / L; (S2) preparing a sodium carbonate solution and adding it dropwise to the metal salt solution to form a reaction solution; (S3) maintaining the pH of the reaction solution between 8.5 and 0.3 and reacting at 55 to 65°C to form a solid product; (S4) allowing the product to cool at room temperature, then removing and washing the solid product; and (S5) calcining the solid product in air at 350 to 550°C to form the indium-based catalyst described above.

[0030] The implementation details and principles of each of the above steps will be described in detail below.

[0031] Please refer to Figure 1 The preparation method of the indium-based catalyst according to an embodiment of the present invention firstly involves: (S1) preparing a metal salt solution with a concentration of 0.25 to 0.55 mol / L. In this step, the metal salt solution contains at least one metal salt, which is formed by dissolving at least one metal salt in water. The metal salt includes indium salt, cobalt salt, and zirconium salt. In one embodiment of the present invention, the indium salt is indium nitrate, the cobalt salt is cobalt nitrate, and the zirconium salt is zirconium nitrate. In one embodiment, the molar ratio of the indium salt to the metal salt is 0.5 to 0.9, and can be 0.5, 0.6, 0.7, 0.8, or 0.8, or other molar ratios between 0.5 and 0.9. In one embodiment, the molar ratio of the cobalt salt to the zirconium salt is less than 10, and can be, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, or other non-integer molar ratios.

[0032] Please refer to Figure 1 The preparation method of the indium-based catalyst in one embodiment of the present invention is as follows: (S2) a sodium carbonate solution is prepared and added dropwise to the metal salt solution to form a reaction solution.

[0033] In this step, the sodium carbonate solution has a concentration of 0.15 to 0.45 mol / L, for example, 0.2, 0.3, or 0.4 mol / L, but is not limited thereto. This step may also include stirring the reaction solution at a speed of 250 to 350 rpm for 0.5 to 2 hours.

[0034] Please refer to Figure 1 The preparation method of the indium-based catalyst according to an embodiment of the present invention then proceeds as follows: (S3) maintaining the pH of the reaction solution between 8.5 and 0.3, and carrying out the reaction at 55 to 65°C to form a solid product. In this step, stirring as in step (S2) may also continue.

[0035] Please refer to Figure 1 The preparation method of the indium-based catalyst according to an embodiment of the present invention then proceeds as follows: (S4) After cooling at room temperature, the solid product is removed and washed. In this step, the reaction solution is cooled to room temperature and aged for 10 to 14 hours, for example, 10, 11, 12, 13, or 14 hours. In this step, the solid product can be obtained by vacuum filtration or centrifugation, and the solid product is washed with deionized water to bring its pH value to neutral or near neutral.

[0036] Preferably, in one embodiment, after washing, the solid product can be dried at 100 to 120°C for 10 to 14 hours before proceeding to the next step.

[0037] Please refer to Figure 1 The preparation method of the indium-based catalyst according to an embodiment of the present invention is then: (S5) calcining the solid product in air at 350 to 550°C to form the above-mentioned indium-based catalyst.

[0038] In this step, the calcination time of the solid product can be 5 to 7 hours.

[0039] To make the indium-based catalyst and its preparation method of the present invention clearer, and to verify the effectiveness of the indium-based catalyst in the catalytic production of methanol from carbon dioxide, the following experiments were conducted.

[0040] Example 1: Calcination temperature 350℃

[0041] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O), 0.6549g of cobalt nitrate hydrate (Co(NO3)2·6H2O), and 0.3220g of zirconium nitrate hydrate (Zr(NO3)4·5H2O), and dissolve them in 50ml of deionized water at room temperature and stir magnetically for 30min to prepare a metal salt solution A. Next, weigh 2.5g of sodium carbonate, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a sodium carbonate solution B. Then, in a beaker C containing 20ml of water, stir at 250-350 rpm in a 60℃ water bath while adding solutions A and B dropwise, maintaining the pH at 8.5±0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10-14 hours.

[0042] After cooling, use deionized water to mix with the precipitate mixture obtained after removing the supernatant during aging, at a ratio of 10:1 (mass ratio), stir for 3 to 5 minutes, then use a centrifuge to separate the solid precipitate. After removing the supernatant, mix the solid precipitate with deionized water again at a ratio of 10:1 (mass ratio) and centrifuge. Wash 5-7 times, replacing the deionized water with ethanol in the last wash. Dry in an oven at 110°C for about 12 hours, then transfer to a muffle furnace and calcine at 350°C with air for 6 hours to obtain the indium-based catalyst.

[0043] Example 2: Calcination temperature 450℃

[0044] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O), 0.6549g of cobalt nitrate hydrate (Co(NO3)2·6H2O), and 0.3220g of zirconium nitrate hydrate (Zr(NO3)4·5H2O), and dissolve them in 50ml of deionized water at room temperature and stir magnetically for 30min to prepare a metal salt solution A. Weigh 2.5g of sodium carbonate, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a sodium carbonate solution B. Then, in a beaker C containing 20ml of water, stir at 250 to 350 rpm in a 60℃ water bath, and add solutions A and B dropwise, maintaining the pH at 8.5±0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10 to 14 hours.

[0045] After cooling, the precipitate obtained after removing the supernatant from the aging process is mixed with deionized water at a ratio of 10:1 (mass ratio). The mixture is stirred for 3 to 5 minutes, and then the precipitate is separated using a centrifuge. After removing the supernatant, the precipitate is mixed with deionized water again at a ratio of 10:1 (mass ratio) and centrifuged. The mixture is washed 5 to 7 times. In the last wash, the deionized water is replaced with ethanol. The mixture is then dried in an oven at 110°C for about 12 hours. Finally, it is transferred to a muffle furnace and calcined at 450°C with air for 6 hours to obtain the indium-based catalyst.

[0046] Example 3: Calcination temperature 550℃

[0047] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O), 0.6549g of cobalt nitrate hydrate (Co(NO3)2·6H2O), and 0.3220g of zirconium nitrate hydrate (Zr(NO3)4·5H2O), and dissolve them in 50ml of deionized water at room temperature and stir magnetically for 30min to prepare a metal salt solution A. Weigh 2.5g of sodium carbonate, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a sodium carbonate solution B. Then, in a beaker C containing 20ml of water, stir at 250 to 350 rpm in a 60℃ water bath, and add solutions A and B dropwise, maintaining the pH at 8.5±0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10 to 14 hours.

[0048] After cooling, the precipitate obtained after removing the supernatant from the aging process is mixed with deionized water at a ratio of 10:1 (mass ratio). The mixture is stirred for 3 to 5 minutes, and then the precipitate is separated using a centrifuge. After removing the supernatant, the precipitate is mixed with deionized water again at a ratio of 10:1 (mass ratio) and centrifuged. The mixture is washed 5 to 7 times. In the last wash, the deionized water is replaced with ethanol. The mixture is then dried in an oven at 110°C for about 12 hours. Finally, it is transferred to a muffle furnace and calcined at 550°C with air for 6 hours to obtain the indium-based catalyst.

[0049] Example 4: Ammonium carbonate as a precipitant

[0050] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O), 0.6549g of cobalt nitrate hydrate (Co(NO3)2·6H2O), and 0.3220g of zirconium nitrate hydrate (Zr(NO3)4·5H2O), and dissolve them in 50ml of deionized water at room temperature and stir magnetically for 30min to prepare a metal salt solution A. Weigh 2.5g of ammonium carbonate, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a precipitant solution B. Then, in a beaker C containing 20ml of water, stir at 60℃ in a water bath at 250 to 350 rpm, and add solutions A and B dropwise, maintaining the pH at 8.5 ± 0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10 to 14 hours.

[0051] After cooling, the precipitate obtained after removing the supernatant during aging is mixed with deionized water at a ratio of 10:1 (mass ratio). The mixture is stirred for 3-5 minutes, then the precipitate is separated using a centrifuge. After removing the supernatant, the precipitate is mixed again with deionized water at a 10:1 (mass ratio) and centrifuged. The mixture is washed 5-7 times, with the deionized water replaced with ethanol in the final wash. The mixture is then dried in an oven at 110°C for approximately 12 hours, followed by calcination in a muffle furnace at 450°C with air for 6 hours. This yields the indium-based catalyst.

[0052] Example 5: Sodium hydroxide as a precipitant

[0053] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O), 0.6549g of cobalt nitrate hydrate (Co(NO3)2·6H2O), and 0.3220g of zirconium nitrate hydrate (Zr(NO3)4·5H2O), and dissolve them in 50ml of deionized water at room temperature and stir magnetically for 30min to prepare a metal salt solution A. Weigh 2.5g of sodium hydroxide, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a precipitant solution B. Then, in a beaker C containing 20ml of water, stir at 250 to 350 rpm in a 60℃ water bath, and add solutions A and B dropwise, maintaining the pH at 8.5 ± 0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10 to 14 hours.

[0054] After cooling, the precipitate obtained after aging and removal of the supernatant is mixed with deionized water at a ratio of 10:1 (mass ratio). The mixture is stirred for 3-5 minutes, then the precipitate is separated using a centrifuge. After removing the supernatant, the precipitate is mixed again with deionized water at a 10:1 (mass ratio) and centrifuged. The mixture is washed 5-7 times, with the last wash using ethanol instead of deionized water. The mixture is then dried in an oven at 110°C for approximately 12 hours, followed by calcination in a muffle furnace at 450°C with air for 6 hours. This yields the indium-based catalyst.

[0055] Example 6:

[0056] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O), 0.5457g of cobalt nitrate hydrate (Co(NO3)2·6H2O), and 0.4830g of zirconium nitrate hydrate (Zr(NO3)4·5H2O), dissolve them in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a metal salt solution A. Weigh 2.5g of sodium carbonate, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a sodium carbonate solution B. Then, place a beaker C containing 20ml of water in a 60℃ water bath and stir at 250 to 350 rpm. Add solutions A and B dropwise, maintaining the pH at 8.5±0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10 to 14 hours.

[0057] After cooling, the precipitate obtained after removing the supernatant from the aging process is mixed with deionized water at a ratio of 10:1 (mass ratio). The mixture is stirred for 3-5 minutes, and then the precipitate is separated using a centrifuge. After removing the supernatant, the precipitate is mixed with deionized water again at a ratio of 10:1 (mass ratio) and centrifuged. The mixture is washed 5-7 times. In the last wash, the deionized water is replaced with ethanol. The mixture is then dried in an oven at 110°C for about 12 hours. Finally, it is transferred to a muffle furnace and calcined at 450°C with air for 6 hours to obtain the indium-based catalyst.

[0058] Example 7:

[0059] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O), 0.7640g of cobalt nitrate hydrate (Co(NO3)2·6H2O), and 0.1610g of zirconium nitrate hydrate (Zr(NO3)4·5H2O), and dissolve them in 50ml of deionized water at room temperature. Stir magnetically for 30min to prepare a metal salt solution A. Weigh 2.5g of sodium carbonate, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a sodium carbonate solution B. Then, place a beaker C containing 20ml of water in a 60℃ water bath and stir at 250 to 350 rpm. Add solutions A and B dropwise, maintaining the pH at 8.5 ± 0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10 to 14 hours.

[0060] After cooling, the precipitate obtained after removing the supernatant from the aging process is mixed with deionized water at a ratio of 10:1 (mass ratio). The mixture is stirred for 3-5 minutes, and then the precipitate is separated using a centrifuge. After removing the supernatant, the precipitate is mixed with deionized water again at a ratio of 10:1 (mass ratio) and centrifuged. The mixture is washed 5-7 times. In the last wash, the deionized water is replaced with ethanol. The mixture is then dried in an oven at 110°C for about 12 hours. Finally, it is transferred to a muffle furnace and calcined at 450°C with air for 6 hours to obtain the indium-based catalyst.

[0061] Example 8:

[0062] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O), 0.4366g of cobalt nitrate hydrate (Co(NO3)2·6H2O), and 0.6440g of zirconium nitrate hydrate (Zr(NO3)4·5H2O), dissolve them in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a metal salt solution A. Weigh 2.5g of sodium carbonate, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a sodium carbonate solution B. Then, place a beaker C containing 20ml of water in a 60℃ water bath and stir at 250 to 350 rpm. Add solutions A and B dropwise, maintaining the pH at 8.5±0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10 to 14 hours.

[0063] After cooling, the precipitate obtained after removing the supernatant from the aging process is mixed with deionized water at a ratio of 10:1 (mass ratio). The mixture is stirred for 3-5 minutes, and then the precipitate is separated using a centrifuge. After removing the supernatant, the precipitate is mixed with deionized water again at a ratio of 10:1 (mass ratio) and centrifuged. The mixture is washed 5-7 times. In the last wash, the deionized water is replaced with ethanol. The mixture is then dried in an oven at 110°C for about 12 hours. Finally, it is transferred to a muffle furnace and calcined at 450°C with air for 6 hours to obtain the indium-based catalyst.

[0064] Comparative Example 9:

[0065] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O) and 1.288g of zirconium nitrate hydrate (Zr(NO3)4·5H2O), dissolve them in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a metal salt solution A. Weigh 2.5g of sodium carbonate, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a sodium carbonate solution B. Then, in a beaker C containing 20ml of water, stir at 250 to 350 rpm in a 60℃ water bath while adding solutions A and B dropwise, maintaining the pH at 8.5 ± 0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10 to 14 hours.

[0066] After cooling, the precipitate obtained after removing the supernatant from the aging process is mixed with deionized water at a ratio of 10:1 (mass ratio). The mixture is stirred for 3-5 minutes, and then the precipitate is separated using a centrifuge. After removing the supernatant, the precipitate is mixed with deionized water again at a ratio of 10:1 (mass ratio) and centrifuged. The mixture is washed 5-7 times. In the last wash, the deionized water is replaced with ethanol. The mixture is then dried in an oven at 110°C for about 12 hours. Finally, it is transferred to a muffle furnace and calcined at 450°C with air for 6 hours to obtain the indium-based catalyst.

[0067] Example 10:

[0068] Weigh 3.61g of indium nitrate hydrate (In(NO3)3·xH2O) and 0.8732g of cobalt nitrate hydrate (Co(NO3)2·6H2O), dissolve them in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a metal salt solution A. Weigh 2.5g of sodium carbonate, dissolve it in 50ml of deionized water at room temperature, and stir magnetically for 30min to prepare a sodium carbonate solution B. Then, in a beaker C containing 20ml of water, stir at 250 to 350 rpm in a 60℃ water bath, and add solutions A and B dropwise, maintaining the pH at 8.5±0.3, until both solutions A and B have been added. After mixing, continue stirring the mixture at the same temperature and speed for 1 hour. After stopping stirring, remove the mixture and allow it to cool and age at room temperature for 10 to 14 hours.

[0069] After cooling, the precipitate obtained after removing the supernatant from the aging process is mixed with deionized water at a ratio of 10:1 (mass ratio). The mixture is stirred for 3-5 minutes, and then the precipitate is separated using a centrifuge. After removing the supernatant, the precipitate is mixed with deionized water again at a ratio of 10:1 (mass ratio) and centrifuged. The mixture is washed 5-7 times. In the last wash, the deionized water is replaced with ethanol. The mixture is then dried in an oven at 110°C for about 12 hours. Finally, it is transferred to a muffle furnace and calcined at 450°C with air for 6 hours to obtain the indium-based catalyst.

[0070] The application method and process parameters of the indium-based catalyst prepared in this invention in a fixed-bed reactor for the hydrogenation of carbon dioxide to methanol are as follows: First, reduction is carried out at 350°C for 6 hours in 10% hydrogen / 90% nitrogen atmosphere, then the temperature is lowered to 200°C in nitrogen atmosphere, and then the feed gas is switched to the feed gas with a feed gas ratio of H2:CO2:N2 = 67.5:22.5:10. Then the temperature and pressure are increased to 240-300°C and 3MPa, and the reaction for the hydrogenation of carbon dioxide to methanol is carried out under certain space velocity conditions.

[0071] Table 1: Effect of different calcination temperatures

[0072]

[0073]

[0074] Table 2: Effects of different precipitants

[0075]

[0076] Table 3: Comparison of different cobalt-zirconium ratios

[0077]

[0078]

[0079] As shown in Table 1-3, at a reaction temperature of 280℃, the indium-based catalyst of this invention, when applied to a fixed-bed reactor for the hydrogenation of carbon dioxide to methanol, exhibited methanol selectivity greater than 45% in all catalyst groups, except for the Indium catalyst used for comparison. 80 Zr 20 Apart from the catalyst, the conversion rates of all groups were greater than 8.5%, indicating that the catalyst of this invention has high catalytic activity and high methanol selectivity. Comparison of the reaction performance of each group shows that the calcination temperature has a relatively small impact on the reaction performance. Furthermore, the ratio of zirconium to cobalt and different precipitants have a significant impact on the catalyst activity and selectivity.

[0080] The present invention has been described by the above-described embodiments; however, these embodiments are merely examples for implementing the present invention. It must be noted that the disclosed embodiments do not limit the scope of the present invention. Conversely, modifications and equivalents contained within the spirit and scope of the claims are included within the scope of the present invention.

Claims

1. A method for preparing an indium-based catalyst for the synthesis of methanol via carbon dioxide hydrogenation, characterized in that: The preparation method includes the following steps: Step (S1): Prepare a metal salt solution containing metal salts, wherein the metal salts are indium salt, cobalt salt and zirconium salt, wherein the indium salt is indium nitrate, the cobalt salt is cobalt nitrate, the zirconium salt is zirconium nitrate, and the concentration of the metal salt solution is 0.25 to 0.55 mol / L; Step (S2): Prepare a sodium carbonate solution and add it dropwise to the metal salt solution to form a reaction solution, wherein the sodium carbonate solution has a concentration of 0.15 to 0.45 mol / L; Step (S3): Maintain the pH of the reaction solution between 8.5 and 0.3, and carry out the reaction at 55 to 65°C to form a solid product; Step (S4): After cooling to room temperature, age for 10 to 14 hours, then remove and wash the solid product; Step (S5): Calcining the solid product in air at 350 to 550°C to form the indium-based catalyst; The indium-based catalyst is an unsupported catalyst containing metal components, namely indium, cobalt, and zirconium. The molar ratio of indium to the metal components is 0.8 to 0.9, and the molar ratio of cobalt to zirconium is less than 10 and not 0.

2. The method for preparing the indium-based catalyst for the synthesis of methanol by carbon dioxide hydrogenation as described in claim 1, characterized in that: The step (S4) further includes drying the solid product at 100 to 120°C for 10 to 14 hours.

3. The method for preparing the indium-based catalyst for the synthesis of methanol by carbon dioxide hydrogenation as described in claim 1, characterized in that: In step (S5), the solid product is calcined for 5 to 7 hours.