A catalyst for synthesizing methanol from oil sludge pyrolysis gasification gas, a preparation method and application thereof

By using silicon carbide, calcium oxide, silicon oxide, and copper-zinc oxide catalysts, the problem of efficiently converting oil sludge pyrolysis gas into methanol was solved, enabling direct methanol synthesis at high temperatures, thus improving economic efficiency and catalyst lifespan.

CN118079972BActive Publication Date: 2026-11-20BEIJING HUANENG CHANGJIANG ENVIRONMENTAL PROTECTION TECH RES INST CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410225904.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2026-11-20
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

In existing technologies, the utilization of oil sludge pyrolysis gasification is extensive and has low added value. The high-temperature gas transportation cost is high and cooling treatment is required, which leads to a decline in economic efficiency. In addition, existing catalysts such as zeolite and precious metal catalysts have problems of deactivation or high cost.

Method used

Using silicon carbide, calcium oxide, and silicon dioxide as the supporting medium, and copper oxide and zinc oxide as the active catalyst, the catalyst is prepared through gradient heat treatment, which is adapted to high-temperature environment for direct synthesis of methanol, avoiding the need for cooling treatment.

Benefits of technology

This improves the resource utilization rate of oil sludge pyrolysis gasification, yielding high-value methanol fuel. The catalyst has good heat resistance and long service life, low cost, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004719617610000061
    Figure BDA0004719617610000061
  • Figure BDA0004719617610000062
    Figure BDA0004719617610000062
Patent Text Reader

Abstract

The application provides a catalyst for synthesizing methanol from oil sludge pyrolysis gasification gas, a preparation method and application thereof. The catalyst comprises a supporting medium and active catalytic catalysts compounded on the surface of the supporting medium. Components of the supporting medium comprise silicon carbide, calcium oxide and silicon dioxide. Components of the active catalytic catalysts comprise copper oxide and zinc oxide. The application selects silicon carbide as a catalytic catalyst dispersion medium, which has excellent high-temperature resistance and can adapt to the high-temperature environment of oil sludge pyrolysis gasification gas. The temperature of the oil sludge pyrolysis gasification gas does not need to be reduced, and the synthesis of methanol can be directly carried out, thereby saving time cost and having high production efficiency. The catalyst has good catalytic effect and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chemical catalyst preparation technology. Specifically, this invention relates to a catalyst for the synthesis of methanol from pyrolysis gasification of oil sludge, its preparation method, and its application. Background Technology

[0002] During the exploration, extraction, refining, tank cleaning, and transportation of petroleum, a large amount of oil sludge is generated. According to its formation, it can be divided into brownish-black ground oil sludge, tank bottom oil sludge containing sand, soil, heavy metal salts, paraffin and asphalt and other heavy oil components deposited at the bottom of oil tanks, oily sludge produced by oil refineries, and oil spills on the ground, which can cause serious damage and threats to the environment.

[0003] Among current technologies for treating oil sludge, pyrolysis gasification is the most favored. This technology, in an oxygen-deficient or anaerobic atmosphere, uses high-temperature heating to cause the oil components in the sludge to undergo decomposition reactions, producing small-molecule high-temperature gases such as CO and H2. Currently, the utilization of this high-temperature gas is relatively rudimentary, mainly through direct incineration. While simple and easy, this method has low added value, and the high transportation costs necessitate the use of nearby incineration facilities. Furthermore, because shut-off valves and other facilities are required before the gas enters the furnace, and to ensure equipment lifespan and operational safety, the high-temperature gas also needs cooling treatment, resulting in a loss of sensible heat carried by the gas and a decrease in economic efficiency. Therefore, developing technologies for utilizing oil sludge pyrolysis gasification gas is essential.

[0004] Methanol is a liquid organic chemical feedstock at room temperature and a core product of one-carbon chemistry, considered an ideal product for the conversion of oil sludge pyrolysis gasification. Therefore, developing a process technology for the catalytic production of methanol from oil sludge pyrolysis gasification, taking into account its characteristics, is of great significance for improving the utilization rate of oil sludge pyrolysis gasification.

[0005] The key to converting oil sludge pyrolysis gas into methanol lies in finding catalysts with high activity, selectivity, and long lifespan. Currently, the most promising catalysts for industrial application are mainly zeolite catalysts and noble metal catalysts, but their limitations are significant due to the easy deactivation of zeolite catalysts and the high cost of noble metal catalysts. Therefore, finding catalysts with high conversion rates of oil sludge pyrolysis gas and high methanol yields, and developing catalytic reaction systems suitable for industrial application, are both hot topics and challenges in the catalytic conversion of oil sludge pyrolysis gas into methanol, and represent a major challenge in catalysis science. Summary of the Invention

[0006] This invention aims to at least partially solve one of the technical problems in related technologies. To this end, embodiments of this invention propose a catalyst for the synthesis of methanol from pyrolysis gasification gas of oil sludge, its preparation method, and its application.

[0007] In a first aspect, embodiments of the present invention provide a catalyst for the synthesis of methanol from pyrolysis gasification gas of oil sludge, the catalyst comprising a supporting medium and an active catalytic catalyst composite on the surface of the supporting medium;

[0008] The components of the loading medium include silicon carbide, calcium oxide, and silicon dioxide;

[0009] The active catalytic catalyst comprises copper oxide and zinc oxide.

[0010] The catalyst in this embodiment of the invention uses silicon carbide as the catalytic catalyst dispersion medium, which has excellent high temperature resistance and can adapt to the high temperature environment of oil sludge pyrolysis gasification gas. It can directly synthesize methanol without lowering the temperature of oil sludge pyrolysis gasification gas, saving time and costs, and has high production efficiency. In addition, the catalyst has good catalytic effect and long service life.

[0011] In some embodiments, the mass ratio of the supporting medium to the active catalytic catalyst is (95-98):(2-5).

[0012] Secondly, embodiments of the present invention also provide a method for preparing the catalyst as described in the first aspect, comprising the following steps:

[0013] (1) Silicon carbide, calcium salt and quartz sand are mixed and ground to obtain a first fine powder, and the first fine powder is mixed with salt water and then shaped to obtain a loaded preform;

[0014] (2) The load blank is subjected to a first gradient heat treatment to obtain the load medium;

[0015] (3) Copper salt and zinc salt are mixed and ground to obtain a second fine powder, and the second fine powder is mixed with anhydrous water to obtain catalyst raw material slurry;

[0016] (4) The catalyst raw material slurry is coated on the surface of the loading medium, and then a second gradient heat treatment is performed to obtain the catalyst.

[0017] The catalyst preparation method of this invention is simple, easy to operate, and uses widely available and inexpensive raw materials, which is conducive to industrial production.

[0018] In some embodiments, in step (1), the particle size of the first fine powder is 60 mesh to 100 mesh;

[0019] And / or, the mass ratio of the silicon carbide, the calcium salt, the quartz sand and the anionized water is (7.5-8.5):(2.5-3.5):(2.5-3.5):(4.5-5.5), preferably 8:3:3:5;

[0020] Preferably, the calcium salt includes at least one of calcium carbonate, calcium sulfate, and calcium nitrate, with calcium carbonate being the most preferred.

[0021] In some embodiments, in step (2), the first gradient heat treatment is carried out under oxygen-free conditions. The firing process is as follows: first, the temperature is raised from room temperature to 850-950°C at a heating rate of 25°C / min and held for 1-2 hours; then, the temperature is raised to 1000-1100°C at a heating rate of 10°C / min and held for 1-2 hours; finally, the temperature is raised to 1200-1300°C at a heating rate of 5°C / min and held for 0.5-1 hour. After cooling, the load medium is obtained.

[0022] In some embodiments, in step (3), the particle size of the second fine powder is 200 mesh to 270 mesh;

[0023] And / or, the mass ratio of the copper salt, the zinc salt and the anhydrous water is (1.5-2.5):(0.5-1.5):(6.5-7.5), preferably 2:1:7;

[0024] Preferably, the copper salt comprises one or a mixture of two of copper sulfate and copper nitrate, preferably copper sulfate; the zinc salt comprises one or a mixture of two of zinc sulfate and zinc nitrate, preferably zinc sulfate.

[0025] In some embodiments, in step (4), the second gradient heat treatment is carried out under oxygen-free conditions. The firing process is as follows: first, the temperature is raised from room temperature to 650-750°C at a heating rate of 20°C / min and held for 1-2 hours; then, the temperature is raised to 950-1050°C at a heating rate of 10°C / min and held for 1-2 hours; finally, the temperature is raised to 1150-1200°C at a heating rate of 5°C / min and held for 2-3 hours. After cooling, the catalyst is obtained.

[0026] Thirdly, the embodiments of the present invention also propose the application of the catalyst as described in the first aspect or the catalyst prepared by the preparation method described in the second aspect in the catalytic reaction of sludge pyrolysis gasification to methanol synthesis.

[0027] The embodiments of the present invention utilize the above-mentioned catalyst to catalyze the synthesis of methanol from the pyrolysis gasification gas of oil sludge, thereby improving the resource utilization of the pyrolysis gasification gas and obtaining methanol fuel, which has high economic value.

[0028] In some embodiments, the composition of the pyrolysis gasification gas of the sludge contains carbon monoxide gas and hydrogen gas, and the reaction temperature of the catalytic reaction is 250-300°C.

[0029] The advantages and beneficial effects of the embodiments of the present invention are as follows:

[0030] (1) In the embodiment of the present invention, silicon carbide is used as the main material in the catalyst support medium. With its excellent heat resistance, the catalyst as a whole can have excellent heat resistance and long service life. At the same time, calcium oxide and silicon dioxide are used as auxiliary materials for the support skeleton, which makes the structure of the support medium more stable and further improves its service life.

[0031] (2) The catalyst preparation method of the present invention uses a variety of raw materials with low cost, the process is simple and easy to operate, and the catalyst has good catalytic effect and long service life, and has a good industrialization prospect. Detailed Implementation

[0032] The embodiments of the present invention are described in detail below. These embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.

[0033] In this document, when values ​​are described as ranges, it should be understood that such disclosure includes disclosure of all possible subranges within that range, as well as the specific numerical values ​​falling within that range, regardless of whether the specific numerical value or specific subrange is explicitly specified.

[0034] In this article, the words “contain” and “include” and their various variations mean that other elements or wholes may be included but not specifically described.

[0035] In this article, the term "and / or" is merely a description of the relationship between related objects, indicating that there can be three kinds of relationships. For example, A and / or B can represent three cases: A exists alone, A and B exist simultaneously, and B exists alone.

[0036] In a first aspect, embodiments of the present invention provide a catalyst for the synthesis of methanol from pyrolysis gasification gas of oil sludge, the catalyst comprising a supporting medium and an active catalytic catalyst composite on the surface of the supporting medium;

[0037] The components of the loading medium include silicon carbide, calcium oxide, and silicon dioxide;

[0038] The active catalytic catalyst comprises copper oxide and zinc oxide.

[0039] This invention employs a mixture of silicon carbide, calcium oxide, and silicon dioxide as the supporting medium. Silicon carbide possesses excellent high-temperature resistance, adapting to the high-temperature environment of oil sludge pyrolysis gasification, which facilitates the direct synthesis of methanol from the pyrolysis gasification gas without the need for cooling, exhibiting strong high-temperature catalytic activity. Calcium oxide serves as a binding component in the framework structure, enhancing the stability of the supported structure. Silicon dioxide provides the supporting medium with good hardness and strength, facilitating transportation and extending its service life. Furthermore, this invention also selects a mixture of copper oxide and zinc oxide as the active catalytic catalyst. Copper oxide is inexpensive to manufacture and possesses good catalytic activity; zinc oxide exhibits excellent catalytic activity and strong selectivity for methanol synthesis. The mixture of these two catalysts directly participates in the methanol synthesis reaction as a high-quality catalyst.

[0040] In some embodiments, the mass ratio of the supporting medium to the active catalytic catalyst is (95-98):(2-5), for example, 95:5, 96:4, 97:3, 97.5:2.5, or 98:2, but is not limited to the listed values; other unlisted values ​​within this range are also applicable. The inventors have discovered that if the mass ratio of the active catalytic catalyst is too high, the catalyst will detach from the supporting surface, and the resulting surface unevenness will affect the catalytic effect; however, if the mass ratio of the catalytic catalyst is too low, the catalyst content will be insufficient, thus reducing the catalytic effect. Therefore, this application controls the mass ratio of the supporting medium to the active catalytic catalyst within the range of (95-98):(2-5).

[0041] Secondly, embodiments of the present invention also provide a method for preparing the catalyst as described in the first aspect, comprising the following steps:

[0042] (1) Silicon carbide, calcium salt and quartz sand are mixed and ground to obtain a first fine powder, and the first fine powder is mixed with salt water and then shaped to obtain a loaded preform;

[0043] (2) The load blank is subjected to a first gradient heat treatment to obtain the load medium;

[0044] (3) Copper salt and zinc salt are mixed and ground to obtain a second fine powder, and the second fine powder is mixed with anhydrous water to obtain catalyst raw material slurry;

[0045] (4) The catalyst raw material slurry is coated on the surface of the loading medium, and then a second gradient heat treatment is performed to obtain the catalyst.

[0046] In some embodiments, in step (1), the particle size of the first fine powder is 60 mesh to 100 mesh, for example, it can be 60 mesh, 70 mesh, 75 mesh, 80 mesh or 100 mesh, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable. This application grinds the raw material powder of the load medium to make its fine powder particle size reach 60 mesh to 100 mesh, which is beneficial to the formation of pores on the surface of the load medium for the catalyst particles to fill.

[0047] And / or, the mass ratio of the silicon carbide, the calcium salt, the quartz sand, and the anhydrous water is (7.5–8.5):(2.5–3.5):(2.5–3.5):(4.5–5.5), for example, it can be 7.5:2.5:2.5:4.5, 7.5:3:3:5, 8:3:3:5, 8:3.2:3.2:5, or 8.5:3.5:3.5:5.5, but is not limited to the listed values; other unlisted values ​​within this range are also applicable; 8:3:3:5 is further preferred; this application introduces anhydrous water as a solvent. The agent has high purity, which ensures that no other impurities are introduced during the preparation of the active catalytic catalyst. In addition, this application controls the mass ratio of silicon carbide, calcium salt, quartz sand and anhydrous water within the range of (7.5~8.5):(2.5~3.5):(2.5~3.5):(4.5~5.5). If the mass ratio of silicon carbide is too high, it will lead to difficulty in forming the loaded preform and high brittleness after firing, making it easy to be damaged during transportation, and the cost will be high. However, if the mass ratio of silicon carbide is too low, it will result in poor heat resistance of the loading medium, and it will be easy to be damaged by thermal deformation during use.

[0048] Furthermore, the calcium salt includes at least one of calcium carbonate, calcium sulfate, and calcium nitrate, preferably calcium carbonate, which is less expensive and more easily decomposes into calcium oxide.

[0049] It should be noted that in step (1), the first fine powder is mixed with the salt water and then shaped by clay molding to obtain the loaded embryo. The shape of the loaded embryo is not particularly limited, and those skilled in the art can prepare it into various shapes according to actual needs, so that it can be applied to different scenarios.

[0050] In some embodiments, in step (2), the first gradient heat treatment is carried out under oxygen-free conditions. The firing process is as follows: first, the temperature is raised from room temperature to 850-950°C at a heating rate of 25°C / min and held for 1-2 hours; then, the temperature is raised to 1000-1100°C at a heating rate of 10°C / min and held for 1-2 hours; finally, the temperature is raised to 1200-1300°C at a heating rate of 5°C / min and held for 0.5-1 hours. After cooling, the load medium can be obtained.

[0051] By subjecting the load preform to gradient heat treatment, calcium salts can be decomposed into calcium oxide at high temperatures. Calcium oxide can serve as a connecting component of the load skeleton, facilitating molding. However, if calcium oxide is directly introduced, it will undergo an exothermic reaction upon mixing with water, which is inconvenient for practical preparation. Therefore, this application uses a calcium salt precursor, which is decomposed at high temperatures to indirectly obtain calcium oxide. Furthermore, this application employs a gradient heat treatment method to perform segmented, step-by-step heating of the load preform, which can prevent deformation and damage to the load preform due to excessively rapid heating and ensure firing efficiency.

[0052] In some embodiments, in step (3), the particle size of the second fine powder is 200 mesh to 270 mesh, for example, it can be 200 mesh, 220 mesh, 240 mesh, 250 mesh or 270 mesh, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable. By finely grinding the raw material powder of the active catalytic catalyst to achieve a particle size of 200 mesh to 270 mesh, it is beneficial to obtain a more uniform catalyst raw material slurry, which can then be uniformly coated on the surface of the loading medium.

[0053] And / or, the mass ratio of the copper salt, the zinc salt, and the anionized water is (1.5-2.5):(0.5-1.5):(6.5-7.5), for example, it can be 1.5:0.5:6.5, 1.5:1:6.8, 2:1:7, 2:1.5:7, or 2.5:1.5:7.5, but is not limited to the listed values, other unlisted values ​​within this range are also applicable; further preferably, it is 2:1:7; and the inventors have found through research that if the mass ratio of copper salt is too high, the catalyst will be easily affected by impurities such as H2S in the pyrolysis gas of oil sludge and be poisoned; but if the mass ratio of copper salt is too low, that is, if the mass ratio of zinc salt is too high, the preparation cost will increase; if the mass ratio of zinc salt is too low, the catalytic activity of the catalyst will decrease. Therefore, this application controls the mass ratio of copper salt to zinc salt to be (1.5-2.5):(0.5-1.5);

[0054] Preferably, the copper salt comprises one or a mixture of two of copper sulfate and copper nitrate, with copper sulfate being more preferred; the zinc salt comprises one or a mixture of two of zinc sulfate and zinc nitrate, with zinc sulfate being more preferred. Compared to nitrates, sulfates are less expensive and have higher solubility; therefore, the copper salt in this application is preferably copper sulfate, and the zinc salt is preferably zinc sulfate.

[0055] In some embodiments, in step (4), the second gradient heat treatment is carried out under oxygen-free conditions. The firing process is as follows: first, the temperature is raised from room temperature to 650-750°C at a heating rate of 20°C / min and held for 1-2 hours; then, the temperature is raised to 950-1050°C at a heating rate of 10°C / min and held for 1-2 hours; finally, the temperature is raised to 1150-1200°C at a heating rate of 5°C / min and held for 2-3 hours. After cooling, the catalyst can be obtained.

[0056] By coating the catalyst raw material slurry onto the surface of the loading medium before firing, the effective components of the catalyst can be more evenly distributed on the surface of the loading medium. Furthermore, after gradient heat treatment, the copper salt in the catalyst raw material slurry decomposes into copper oxide, and the zinc salt decomposes into zinc oxide, thus forming the catalyst components, which directly participate in the methanol synthesis reaction. In addition, gradient heat treatment helps to avoid thermal deformation of the loading medium.

[0057] Thirdly, the embodiments of the present invention also propose the application of the catalyst as described in the first aspect or the catalyst prepared by the preparation method described in the second aspect in the catalytic reaction of sludge pyrolysis gasification to methanol synthesis.

[0058] In some embodiments, the composition of the sludge pyrolysis gasification gas contains carbon monoxide gas and hydrogen gas, and the reaction temperature of the catalytic reaction is 250-300°C, for example, 250°C, 265°C, 270°C, 280°C or 300°C, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0059] When the above catalyst is used in the reaction of pyrolysis gasification of oil sludge to synthesize methanol, the reaction process is as follows:

[0060]

[0061]

[0062] The following are non-limiting embodiments and comparative examples of the present invention. It should be noted that the schemes in the comparative examples are not prior art, but are only set up for comparison with the schemes in the embodiments, and are not intended to limit the present invention. Unless otherwise stated, all raw materials used in the embodiments and comparative examples are conventional commercially available products, or can be prepared by known methods.

[0063] Example 1

[0064] A method for preparing a catalyst for the synthesis of methanol from pyrolysis gasification gas of oil sludge includes the following steps:

[0065] (1) Mix and grind silicon carbide, calcium carbonate and quartz sand until the particle size of the mixed powder reaches 60 mesh, and then mix it evenly with anhydrous salt water and shape it to obtain a loaded preform; wherein, the mass ratio of silicon carbide, calcium carbonate, quartz sand and anhydrous salt water is 8:3:3:5.

[0066] (2) The load blank is placed in a muffle furnace and fired under oxygen-free conditions. The firing process is as follows: first, the temperature is raised from room temperature to 900℃ at a heating rate of 25℃ / min and held for 1h; then the temperature is raised to 1100℃ at a heating rate of 10℃ / min and held for 1h; finally, the temperature is raised to 1200℃ at a heating rate of 5℃ / min and held for 0.5h. After cooling, the load medium is obtained. Among them, calcium carbonate will decompose into calcium oxide and water after high-temperature firing (i.e., CaCO3→CaO+H2O).

[0067] (3) Mix and grind copper sulfate and zinc sulfate until the particle size of the mixed powder reaches 200 mesh, and then mix it evenly with the salt water to obtain catalyst raw material slurry; wherein the mass ratio of copper sulfate, zinc sulfate and salt water is 2:1:7.

[0068] (4) The catalyst raw material slurry obtained in step (3) is coated on the surface of the loading medium obtained in step (2), and then sent to a high-temperature furnace to be fired in the absence of oxygen. The firing process is as follows: first, the temperature is raised from room temperature to 700℃ at a heating rate of 20℃ / min and held for 1h; then the temperature is raised to 1000℃ at a heating rate of 10℃ / min and held for 1h; finally, the temperature is raised to 1180℃ at a heating rate of 5℃ / min and held for 2h. After cooling, a catalyst for the synthesis of methanol from pyrolysis gasification of oil sludge can be obtained. Among them, after high-temperature firing, copper sulfate will decompose into copper oxide and sulfur trioxide, and zinc sulfate will decompose into zinc oxide and sulfur trioxide (i.e.: CuSO4→CuO+SO3; ZnSO4→ZnO+SO3).

[0069] Example 2

[0070] The preparation method of this embodiment is basically the same as that of Example 1, except that in step (1), the mass ratio of silicon carbide, calcium carbonate, quartz sand and salt water is 7.5:3:3:5.

[0071] Example 3

[0072] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that in step (1), the particle size of the mixed powder of silicon carbide, calcium carbonate and quartz sand after grinding is 80 mesh; and the mass ratio of silicon carbide, calcium carbonate, quartz sand and salt water is 8:3.2:3.2:5.

[0073] Example 4

[0074] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that in step (2), the firing process of the first gradient heat treatment is as follows: first, the temperature is raised from room temperature to 900℃ at a heating rate of 25℃ / min and held for 1.5h; then the temperature is raised to 1000℃ at a heating rate of 10℃ / min and held for 2h; finally, the temperature is raised to 1200℃ at a heating rate of 5℃ / min and held for 1h before cooling.

[0075] Example 5

[0076] The preparation method of this embodiment is basically the same as that of Example 1, except that in step (3), the mass ratio of copper sulfate, zinc sulfate and salt water is 1.5:1:6.8.

[0077] Example 6

[0078] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that in step (3), the particle size of the mixed powder of copper sulfate and zinc sulfate after grinding is 250 mesh; and the mass ratio of copper sulfate, zinc sulfate and anhydrous water is 2:1.5:7.

[0079] Example 7

[0080] The preparation method of this embodiment is basically the same as that of Example 1. The difference is that in step (4), the firing process of the second gradient heat treatment is as follows: first, the temperature is raised from room temperature to 650°C at a heating rate of 20°C / min and held for 1.5h; then the temperature is raised to 1000°C at a heating rate of 10°C / min and held for 1.5h; finally, the temperature is raised to 1200°C at a heating rate of 5°C / min and held for 2h before cooling.

[0081] Comparative Example 1

[0082] The preparation method of this comparative example is basically the same as that of Example 1, except that in step (1), the raw material components of the loading medium do not contain silicon carbide.

[0083] Comparative Example 2

[0084] The preparation method of this comparative example is basically the same as that of Example 1. The difference is that in step (2), the first heat treatment process is as follows: the load blank is directly heated to 1200℃ at a heating rate of 10℃ / min, held for 2.5h and then cooled.

[0085] Comparative Example 3

[0086] The preparation method of this comparative example is basically the same as that of Example 1, except that in step (3), the catalyst raw material components do not contain zinc sulfate.

[0087] Comparative Example 4

[0088] The preparation method of this comparative example is basically the same as that of Example 1. The difference is that in step (4), the second heat treatment process is as follows: the loading medium coated with catalyst raw material slurry on the surface is directly heated to 1180°C at a heating rate of 10°C / min, kept at the temperature for 4 hours and then cooled.

[0089] The catalysts prepared in the above examples and comparative examples were used in the reaction process of synthesizing methanol from sludge pyrolysis gasification gas (reaction temperature 250℃, pressure 7.5MPa, inlet gas composition H2:CO:CO2=70:24:6). The performance evaluation results of each catalyst are shown in Table 1:

[0090] Table 1

[0091] CO conversion rate / % Catalyst lifetime / h Example 1 30.6 ~5000 Example 2 30.7 ~4500 Example 3 31.1 ~5000 Example 4 30.5 ~6000 Example 5 32.5 ~5000 Example 6 33.0 ~5000 Example 7 30.9 ~6000 Comparative Example 1 29.3 ~2800 Comparative Example 2 30.5 ~3800 Comparative Example 3 26.2 ~5000 Comparative Example 4 30.4 ~3500

[0092] As shown in Table 1, compared with the catalyst prepared in the comparative example, the catalyst prepared by the segmented gradient heating heat treatment method in the embodiment of the present invention has a longer service life. The data results in Table 1 also show that as the proportion of zinc sulfate added increases, the conversion rate of CO by the catalyst is higher, indicating that its catalytic performance is better. Furthermore, using a higher proportion of silicon carbide results in a longer catalyst service life.

[0093] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0094] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.

Claims

1. A catalyst for the synthesis of methanol from pyrolysis gasification gas of oil sludge, characterized in that, The catalyst includes a supporting medium and an active catalytic catalyst composited on the surface of the supporting medium; the mass ratio of the supporting medium to the active catalytic catalyst is (95-98):(2-5); the supporting medium comprises silicon carbide, calcium oxide and silicon dioxide; the active catalytic catalyst comprises copper oxide and zinc oxide; the pyrolysis gasification gas of the oil sludge contains carbon monoxide gas and hydrogen gas. The catalyst is prepared by a method comprising the following steps: (1) Silicon carbide, calcium salt and quartz sand are mixed and ground to obtain a first fine powder with a particle size of 60 to 100 mesh, and the first fine powder is mixed with anhydrous water and shaped to obtain a loaded preform; wherein, the mass ratio of silicon carbide, calcium salt, quartz sand and anhydrous water is (7.5 to 8.5):(2.5 to 3.5):(2.5 to 3.5):(4.5 to 5.5); (2) The loading preform is subjected to a first gradient heat treatment to obtain the loading medium; the first gradient heat treatment is carried out under oxygen-free conditions, and the firing process is as follows: first, the temperature is raised from room temperature to 850-950℃ at a heating rate of 25℃ / min and held for 1-2 hours; then the temperature is raised to 1000-1100℃ at a heating rate of 10℃ / min and held for 1-2 hours; finally, the temperature is raised to 1200-1300℃ at a heating rate of 5℃ / min and held for 0.5-1 hours, and the loading medium is obtained after cooling. (3) Copper salt and zinc salt are mixed and ground to obtain a second fine powder with a particle size of 200-270 mesh, and the second fine powder is mixed with anhydrous water to obtain catalyst raw material slurry; (4) The catalyst raw material slurry is coated on the surface of the loading medium, and then a second gradient heat treatment is performed to obtain the catalyst. The second gradient heat treatment is carried out under oxygen-free conditions. The firing process is as follows: first, the temperature is raised from room temperature to 650-750°C at a heating rate of 20°C / min and held for 1-2 hours; then, the temperature is raised to 950-1050°C at a heating rate of 10°C / min and held for 1-2 hours; finally, the temperature is raised to 1150-1200°C at a heating rate of 5°C / min and held for 2-3 hours.

2. The catalyst according to claim 1, characterized in that, In step (1), the calcium salt includes at least one of calcium carbonate, calcium sulfate, and calcium nitrate.

3. The catalyst according to claim 1, characterized in that, In step (1), the mass ratio of silicon carbide, calcium salt, quartz sand and anhydrous water is 8:3:3:

5.

4. The catalyst according to claim 1, characterized in that, In step (3), the mass ratio of the copper salt, the zinc salt and the anionless water is (1.5-2.5):(0.5-1.5):(6.5-7.5); the copper salt includes one or a mixture of copper sulfate and copper nitrate; the zinc salt includes one or a mixture of zinc sulfate and zinc nitrate.

5. The application of the catalyst according to any one of claims 1-4 in the catalytic reaction of sludge pyrolysis gasification to methanol synthesis.

6. The application according to claim 5, characterized in that, The reaction temperature of the catalytic reaction is 250–300°C.

Citation Information

Patent Citations

  • Method for promoting forming of aurichalcite phase in precursor of copper-based catalyst with calcium salt as additive

    CN105664954A

  • Catalyst, and preparation method and application thereof

    CN106492814A

  • Preparation method of sorbitol

    CN117603009A