Process for recovering copper and sulfur from high-sulfur low-grade copper ore by pre-tailing

By combining pre-screening and magnetic-gravity separation with ball milling and flotation, the problems of high cost and low sulfur recovery rate of low-grade copper ore were solved, achieving efficient recovery of copper and sulfur, reducing production costs and improving concentrate grade.

CN118080152BActive Publication Date: 2026-11-20SU NI TE YOU QI ZHU RI HE TONG YE YOU XIAN ZE REN GONG SI +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410440680.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2026-11-20
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

Existing low-grade copper sulfide beneficiation processes are costly and have low sulfur recovery rates, while existing pre-tailings removal technologies have high investment costs and strict requirements on material layer thickness.

Method used

The raw ore is pre-screened to remove coarse particles. The tailings are then removed in advance using magnetic separation and gravity separation. The tailings are then combined with jigging gravity separation, followed by ball milling and preferential copper flotation. Copper and sulfur are then separated. The pH of the slurry is controlled at 8–8.5 using a low-alkalinity sulfur inhibitor. The copper tailings are then preferentially flotated and sulfur is further separated.

Benefits of technology

It achieves efficient recovery of copper and sulfur from high-sulfur, low-grade copper ores with low investment and low cost, with copper recovery rate ≥80% and sulfur recovery rate ≥92%, reducing subsequent grinding and beneficiation costs and improving concentrate grade.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118080152B_ABST
    Figure CN118080152B_ABST
Patent Text Reader

Abstract

The application relates to a process for pre-throwing tailings to recover copper and sulfur in low-grade copper ore, wherein the low-grade copper ore is crushed, the material above the 0.3mm sieve is subjected to magnetic separation by a magnetic separator to obtain a magnetic separation concentrate and a magnetic separation tailings, the magnetic separation tailings are subjected to gravity separation by a jig to obtain jig concentrate and jig tailings, the jig concentrate and the magnetic separation concentrate are mixed and then are subjected to grinding together with the material below the sieve by a ball mill, the ground material is subjected to copper selection and then sulfur flotation, a sulfur inhibitor, No.2 oil and Z200 are added in the copper rough selection to obtain copper concentrate, the pH of the slurry is 8-8.5, and the copper concentrate is obtained through once copper cleaning, twice copper cleaning and thrice copper cleaning; the sulfur inhibitor is added in the once copper cleaning and the twice copper cleaning, the tailings after once scavenging are subjected to sulfur rough selection, and sulfur concentrate is obtained through once sulfur scavenging and twice sulfur scavenging; the sulfur inhibitor, No.2 oil and sulfuric acid are added in the sulfur rough selection, and the sulfur inhibitor is added in the once sulfur scavenging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of mineral processing, and in particular to a process for pre-discarding tailings to recover copper and sulfur from high-sulfur, low-grade copper ore. Background Technology

[0002] In existing low-grade copper sulfide beneficiation processes, grinding and classification are usually followed by direct flotation. When the grade of the raw ore is low, the beneficiation cost is relatively high. Existing pre-tailings removal technology mostly uses intelligent sorting equipment, but its disadvantages are that it has strict requirements on the thickness of the material layer and the investment cost is relatively high.

[0003] Patent CN103386356A discloses a flotation method for copper sulfide ore, comprising the following steps: (1) grinding the copper sulfide ore in a primary stage to obtain a primary grinding product containing at least 65% particles smaller than 200 mesh; (2) performing a first flotation on the primary grinding product using a first trapping agent to obtain a first flotation product containing single copper minerals and secondary copper-rich mineral intergrowths, and a first flotation residue; (3) performing a second flotation on the first flotation residue using a second trapping agent to obtain a second flotation product containing copper-poor intergrowths, complex copper minerals, and single sulfur, and a second flotation tailings; (4) performing a second stage grinding on the second flotation product to obtain a second stage grinding product containing at least 85% particles smaller than 325 mesh; and (5) separating copper and sulfur in the second stage grinding product in a strongly alkaline environment to obtain copper concentrate and sulfur concentrate. This patent has a high flotation alkalinity, which can damage flotation equipment. The sulfur recovery rate is also low. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a process for pre-disposal of tailings to recover copper and sulfur from high-sulfur, low-grade copper ore, which has low investment, low cost, and high recovery rate.

[0005] To achieve the above objectives, the present invention employs the following technical solution:

[0006] A process for pre-disposal recovery of copper and sulfur from high-sulfur, low-grade copper ore involves pre-screening coarse-grained raw ore and using magnetic separation for pre-disposal. Specifically, the low-grade copper ore is crushed to below 5mm and then screened using a 0.3mm sieve. The oversize material is then magnetically separated to obtain magnetic concentrate and magnetic tailings. The magnetic tailings are then gravity-separated using a jig to obtain jigging concentrate and jigging tailings. The jigging concentrate and magnetic concentrate are mixed and then ground together with the undersize material using a ball mill. After grinding, the material is preferentially selected for copper flotation followed by sulfur flotation. In the copper flotation, sulfur inhibitors, No. 2 oil, and Z200 are added for copper roughing. The pulp pH is 8-8.5. The copper concentrate is then obtained through primary, secondary, and tertiary copper cleaning. Sulfur inhibitors are added in both primary and secondary copper cleaning. In the sulfur flotation, the tailings after primary scavenging are subjected to sulfur roughing, primary sulfur scavenging, and secondary sulfur scavenging to obtain sulfur concentrate. Xanthate, No. 2 oil, and sulfuric acid are added in the sulfur roughing, and xanthate is added in the primary sulfur scavenging.

[0007] The high-sulfur, low-grade copper ore is a pyrrhotite-bearing ore with a copper grade ≤0.60% and a sulfur grade ≥19%.

[0008] The magnetic separation field strength is 0.8 to 1 T.

[0009] The jig conditions are: stroke 20mm, stroke rate 260r / min.

[0010] The sulfur inhibitor is prepared by mixing lime, ammonium persulfate, zinc sulfate, and sodium sulfite in a mass ratio of 10-12:1:2-2.5:1-1.5.

[0011] The secondary sulfur scavenging concentrate is returned to the primary sulfur scavenging process, and the final sulfur roughing concentrate and the primary sulfur scavenging concentrate are mixed to obtain sulfur concentrate.

[0012] In the copper roughing process, the dosage of sulfur inhibitor is 80-100 g / t, the dosage of Z200 is 60-80 g / t, and the dosage of No. 2 oil is 10-20 g / t.

[0013] The amount of sulfur inhibitor used in the copper beneficiation process is 60-80 g / t.

[0014] The amount of sulfur inhibitor used in the secondary copper beneficiation process is 8-10 g / t.

[0015] The amount of sulfur crude yellow medicine used is 20-30 g / t; the amount of No. 2 oil used is 10-20 g / t; and the amount of sulfuric acid used is 200-300 g / t.

[0016] The dosage of yellow yam in the single sulfur scavenging is 10-15 g / t.

[0017] After beneficiation, copper concentrate with a copper grade of 19%–23% and sulfur concentrate with a sulfur grade of 38%–42% are obtained.

[0018] Compared with existing technologies, the beneficial effects of this invention are:

[0019] 1. This process pre-discards the coarse-grained ore, using magnetic separation for early tailings disposal. Gravity separation is then used to recover some copper- and sulfur-containing minerals from the magnetic tailings. This pre-discarding of tailings reduces subsequent grinding and beneficiation costs. The recovery of copper sulfide ore containing pyrrhotite employs a mining-benefit + gravity separation method, which has the advantages of low investment and low production costs.

[0020] 2. The process involves preferential flotation of copper, followed by sulfur removal from copper tailings. Preferential flotation is characterized by a stable and easily controllable flotation process and a high concentrate grade.

[0021] 3. The sulfur inhibitor in this application is a low-alkalinity sulfur inhibitor. Currently, conventional copper-sulfur separation uses inhibitors with high alkalinity, resulting in a pulp pH of 10-11 after use. However, using the sulfur inhibitor in this application lowers the pulp flotation pH to 8-8.5, effectively reducing the amount of sulfuric acid used in subsequent sulfur beneficiation and lowering beneficiation costs. Simultaneously, it has a good sulfur inhibition effect, ensuring the grade of copper concentrate. Lime provides an alkaline environment, which has an inhibitory effect on sulfide ores under alkaline conditions. Ammonium persulfate has strong oxidizing properties, which can strengthen sulfur and thus inhibit its floatability. Zinc sulfate has the best inhibitory effect on sulfide ores under alkaline conditions and has a selective inhibitory effect on sulfide ores. Sodium sulfite has a good selective inhibitory effect, a smaller inhibitory effect on chalcopyrite, and a good inhibitory effect on pyrite.

[0022] 4. The copper recovery rate of the process in this application is ≥80%, and the sulfur recovery rate is ≥92%. The copper grade of the copper concentrate is ≥19%, and the sulfur grade of the sulfur concentrate is ≥38% (S+Fe≥90%). Attached Figure Description

[0023] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation

[0024] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other.

[0025] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are used only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this invention, unless otherwise stated, "a plurality of" means two or more.

[0026] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art will understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0027] like Figure 1 A process for pre-disposal recovery of copper and sulfur from high-sulfur, low-grade copper ore involves pre-screening coarse-grained raw ore and using magnetic separation for pre-disposal. Specifically, the low-grade copper ore is crushed to below 5mm and then screened using a 0.3mm sieve. The oversize material is then magnetically separated to obtain magnetic concentrate and magnetic tailings. The magnetic tailings are then gravity separated using a jig to obtain jigging concentrate and jigging tailings. The jigging concentrate and magnetic concentrate are mixed and then ground together with the undersize material in a ball mill. The ground material is then subjected to flotation for copper removal followed by sulfur removal. In copper beneficiation, sulfur inhibitors, No. 2 oil, and Z200 are added for roughing. The pulp pH is reduced to 8-8.5. The copper concentrate is then obtained through primary copper cleaning (refinery 1), secondary copper cleaning (refinery 2), and tertiary copper cleaning (refinery 3). Sulfur inhibitors are added to both primary and secondary copper cleaning (refinery 1). In sulfur beneficiation, tailings from primary scavenging (scavenging 1) undergo sulfur roughing, primary sulfur scavenging (scavenging 1-1), and secondary sulfur scavenging (scavenging 2-1). Xanthate, No. 2 oil, and sulfuric acid are added to the sulfur roughing, while xanthate is added to the primary sulfur scavenging (scavenging 1-1). The concentrate from the secondary sulfur scavenging (scavenging 2-1) is returned to the primary sulfur scavenging. Finally, the sulfur roughing concentrate and the primary sulfur scavenging concentrate are mixed to obtain the sulfur concentrate.

[0028] The aforementioned low-grade copper ore has a copper grade of ≤0.60% and a sulfur grade of ≤19%.

[0029] The magnetic separation field strength is 0.8 to 1 T.

[0030] The jig conditions are: stroke 20mm, stroke rate 260r / min.

[0031] The sulfur inhibitor is prepared by mixing lime, ammonium persulfate, zinc sulfate, and sodium sulfite in a mass ratio of (10-12):1:(2-2.5):(1-1.5).

[0032] In the copper roughing process, the dosage of sulfur inhibitor is 80-100 g / t, the dosage of Z200 is 60-80 g / t, and the dosage of No. 2 oil is 10-20 g / t.

[0033] The amount of sulfur inhibitor used in the copper beneficiation process is 60-80 g / t.

[0034] The amount of sulfur inhibitor used in the secondary copper beneficiation process is 8-10 g / t.

[0035] The amount of sulfur crude yellow medicine used is 20-30 g / t; the amount of No. 2 oil used is 10-20 g / t; and the amount of sulfuric acid used is 200-300 g / t.

[0036] The dosage of yellow yam in the single sulfur scavenging is 10-15 g / t.

[0037] After beneficiation, copper concentrate with a copper grade ≥19% and sulfur concentrate with a sulfur grade ≥38% (S+Fe≥90%) were obtained.

[0038] Copper recovery rate ≥82%, sulfur recovery rate ≥92%.

[0039] The preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solutions of the present invention, and these simple modifications all fall within the protection scope of the present invention. Furthermore, it should be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not describe the various possible combinations separately. In addition, various different embodiments of the present invention can also be arbitrarily combined, as long as they do not violate the spirit of the present invention, and should also be considered as the content disclosed by the present invention.

[0040] To make the objectives, technical solutions, and technical effects of this invention clearer, the technical solutions in the embodiments of this invention are now described clearly and completely. However, the embodiments described below are only some embodiments of this invention, not all embodiments. All other embodiments obtained by those skilled in the art in conjunction with the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0041] Example 1

[0042] A process for pre-disposal of tailings to recover copper and sulfur from high-sulfur, low-grade copper ore involves pre-screening coarse-grained raw ore and using magnetic separation for pre-disposal of tailings. The raw ore has a copper grade of 0.50% and a sulfur grade of 18.45%.

[0043] Low-grade copper ore is crushed to below 5mm, then screened using a 0.3mm sieve. The oversize material is then subjected to magnetic separation using a 0.8T magnetic separator to obtain magnetic concentrate and tailings. The tailings are then subjected to gravity separation using a jig with the following parameters: stroke 20mm, stroke rate 260r / min. This yields jigged concentrate and jigged tailings.

[0044] The jig concentrate and magnetic separator concentrate are mixed and ground together with the undersize material in a ball mill. The ground material is then preferentially selected for copper flotation followed by sulfur flotation. In the copper flotation process, 100 g / t of sulfur inhibitor, 15 g / t of No. 2 oil, and 70 g / t of Z200 are added for roughing, reducing the pulp pH to 8.3–8.5. The pulp then undergoes primary copper cleaning (cleaner 1), secondary copper cleaning (cleaner 2), and tertiary copper cleaning (cleaner 3) to obtain copper concentrate. In the primary copper cleaning, 65 g / t of sulfur inhibitor is added, resulting in a pulp pH of 8.2–8.4. In the secondary copper cleaning (cleaner 2), 10 g / t of sulfur inhibitor is added, resulting in a pulp pH of 8.0–8.2.

[0045] In the sulfur beneficiation process, the tailings from the first scavenging (Scavenging 1) undergo sulfur roughing, a first sulfur scavenging (Scavenging 1-1), and a second sulfur scavenging (Scavenging 2-1). In the sulfur roughing, 25 g / t of xanthate, 15 g / t of No. 2 oil, and 230 g / t of sulfuric acid are added. In the first sulfur scavenging, 10 g / t of these additives are added. The concentrate from the second sulfur scavenging (Scavenging 2-1) is returned to the first sulfur scavenging (Scavenging 1-1). Finally, the sulfur roughing concentrate and the first sulfur scavenging (Scavenging 1-1) concentrate are mixed to obtain the sulfur concentrate.

[0046] The sulfur inhibitors for copper roughing, primary copper cleaning, and primary copper cleaning are prepared by mixing lime, ammonium persulfate, zinc sulfate, and sodium sulfite in a mass ratio of 10:1:2:1.

[0047] In this embodiment, the copper recovery rate was 82.22% and the sulfur recovery rate was 92.57%. The beneficiation results are shown in Table 1.

[0048] Table 1:

[0049]

[0050] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

[0051] Example 2

[0052] A process for pre-disposal recovery of copper and sulfur in high-sulfur, low-grade copper ore involves pre-screening coarse-grained raw ore and using magnetic separation for pre-disposal of tailings. The raw ore has a copper grade of 0.48% and a sulfur grade of 18.12%.

[0053] Low-grade copper ore is crushed to below 5mm, then screened using a 0.3mm sieve. The oversize material is then subjected to magnetic separation using a 1T magnetic separator to obtain magnetic concentrate and tailings. The tailings are then subjected to gravity separation using a jig with the following parameters: stroke 20mm, stroke rate 260r / min. This yields jigged concentrate and jigged tailings.

[0054] The jigging concentrate and magnetic separation concentrate are mixed and ground together with the undersize material in a ball mill. The ground material is preferentially selected for copper flotation and then for sulfur flotation. In the copper flotation, 90 g / t of sulfur inhibitor, 18 g / t of No. 2 oil and 75 g / t of Z200 are added for copper roughing. The pH of the pulp is reduced to 8.3-8.5. Then, copper concentrate is obtained by primary copper cleaning (refinery 1), secondary copper cleaning (refinery 2) and tertiary copper cleaning (refinery 3). The sulfur inhibitor dosage for primary copper cleaning is 80 g / t, and the pulp pH is 8.2-8.4. The sulfur inhibitor dosage for secondary copper cleaning (refinery 2) is 9 g / t, and the pulp pH is 8.0-8.2.

[0055] In the sulfur beneficiation process, the tailings from the first scavenging (Scavenging 1) undergo sulfur roughing, a first sulfur scavenging (Scavenging 1-1), and a second sulfur scavenging (Scavenging 2-1). In the sulfur roughing, 28 g / t of xanthate, 12 g / t of No. 2 oil, and 220 g / t of sulfuric acid are added. In the first sulfur scavenging, 12 g / t of these additives are added. The concentrate from the second sulfur scavenging (Scavenging 2-1) is returned to the first sulfur scavenging (Scavenging 1-1). Finally, the sulfur roughing concentrate and the first sulfur scavenging (Scavenging 1-1) concentrate are mixed to obtain the sulfur concentrate.

[0056] The sulfur inhibitors for copper roughing, primary copper cleaning, and primary copper cleaning are prepared by mixing lime, ammonium persulfate, zinc sulfate, and sodium sulfite in a mass ratio of 11:1:2.2:1.2.

[0057] In this embodiment, the copper recovery rate was 86.31% and the sulfur recovery rate was 92.60%. The beneficiation results are shown in Table 2.

[0058]

Claims

1. A process for pre-disposal recovery of copper and sulfur from high-sulfur, low-grade copper ore, characterized in that, Coarse-grained raw ore is pre-screened and tailings are disposed of early using magnetic separation. Specifically, low-grade copper ore is crushed to below 5mm and then screened using a 0.3mm sieve. The oversize material is then magnetically separated to obtain magnetic concentrate and tailings. The magnetic tailings are then gravity separated using a jig to obtain jigging concentrate and tailings. The jigging concentrate and magnetic concentrate are mixed and ground together with the undersize material using a ball mill. The ground material is then subjected to copper flotation first and then sulfur flotation. In the copper flotation, sulfur inhibitors, No. 2 oil, and Z200 are added for copper roughing. The pulp pH is 8-8.

5. The copper concentrate is then obtained through primary, secondary, and tertiary copper cleaning. Sulfur inhibitors are added in both primary and secondary copper cleaning. In the sulfur flotation, the tailings from the primary scavenging are subjected to sulfur roughing, primary sulfur scavenging, and secondary sulfur scavenging to obtain sulfur concentrate. Xanthium, No. 2 oil, and sulfuric acid are added in the sulfur roughing, and xanthium is added in the primary sulfur scavenging. The sulfur inhibitor is prepared by mixing lime, ammonium persulfate, zinc sulfate, and sodium sulfite in a mass ratio of 10-12:1:2-2.5:1-1.

5.

2. The process for pre-disposal recovery of copper and sulfur from high-sulfur, low-grade copper ore according to claim 1, characterized in that, The high-sulfur, low-grade copper ore is a pyrrhotite-bearing ore with a copper grade ≤0.60% and a sulfur grade ≥19%.

3. The process for pre-disposal recovery of copper and sulfur from high-sulfur, low-grade copper ore according to claim 1, characterized in that, The magnetic separation field strength is 0.8 to 1 T.

4. The process for pre-disposal recovery of copper and sulfur from high-sulfur, low-grade copper ore according to claim 1, characterized in that, The jig conditions are: stroke 20mm, stroke rate 260r / min.

5. The process for pre-disposal recovery of copper and sulfur from high-sulfur, low-grade copper ore according to claim 1, characterized in that, The secondary sulfur scavenging concentrate is returned to the primary sulfur scavenging process, and the final sulfur roughing concentrate and the primary sulfur scavenging concentrate are mixed to obtain sulfur concentrate.

6. The process for pre-disposal recovery of copper and sulfur from high-sulfur, low-grade copper ore according to claim 1, characterized in that, In the copper roughing process, the dosage of sulfur inhibitor is 80-100 g / t, Z200 dosage is 60-80 g / t, and No. 2 oil dosage is 10-20 g / t; in the primary copper beneficiation process, the dosage of sulfur inhibitor is 60-80 g / t; in the secondary copper beneficiation process, the dosage of sulfur inhibitor is 8-10 g / t; in the sulfur roughing process, the dosage of yellowing agent is 20-30 g / t; in the No. 2 oil process, the dosage is 10-20 g / t; in the sulfuric acid process, the dosage is 200-300 g / t; and in the primary sulfur scavenging process, the dosage of yellowing agent is 10-15 g / t.

7. The process for pre-disposal recovery of copper and sulfur from high-sulfur, low-grade copper ore according to claim 1, characterized in that, After beneficiation, copper concentrate with a copper grade of 19%–23% and sulfur concentrate with a sulfur grade of 38%–42% are obtained.

Citation Information

Patent Citations

  • Flotation method for copper sulphide ore

    CN103386356A

  • Fine grinding and comprehensive recycling beneficiation process of copper-containing sulfur concentrate

    CN105327771A

  • Beneficiation method for diversified raw ore

    CN108906312A