A method for producing 60-50kg / m U75V special-shaped steel rails without normalizing heat treatment

By utilizing the residual heat of the rail during the forging process to separately control the cooling of the forming section, transition section, and heat-affected zone of the shaped rail with air jets, the problems of abnormal structure and excessive hardness caused by traditional normalizing heat treatment are solved. This achieves high strength and high hardness for the shaped rail, simplifies the production process, and reduces costs.

CN118080772BActive Publication Date: 2026-11-24BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311325469.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-12
Publication Date
2026-11-24
Estimated Expiration
2043-10-12

AI Technical Summary

Technical Problem

In the production of 60-50kg/m U75V special-shaped steel rails, the traditional normalizing heat treatment has problems such as unsuitable cooling temperature, increased production cost and difficulty in control, and may lead to abnormal structure and excessive hardness.

Method used

The residual heat from the forging process is utilized to separately control the cooling of the forming section, transition section, and heat-affected zone of the special-shaped rail by spraying air. Normalizing heat treatment is omitted, and the focus is on spraying air to cool the top and sides of the rail head, controlling the cooling rate and temperature.

Benefits of technology

It improves the strength and hardness of the rails, refines the microstructure, simplifies the production process, reduces energy consumption and labor costs, and meets the mechanical performance requirements of special-shaped rails.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118080772B_ABST
    Figure CN118080772B_ABST
Patent Text Reader

Abstract

This invention discloses a method for producing 60-50kg / m U75V special-shaped steel rails without normalizing heat treatment. The process includes the following steps: blanking → forging → shot blasting → straightening → milling → fine adjustment → length setting → drilling → flaw detection → finished product. This method eliminates the traditional normalizing heat treatment after forging; instead, it utilizes the residual heat from the forging process to control the cooling of the forming section, transition section, and heat-affected zone of the special-shaped steel rail. The mechanical properties of the 60-50kg / m U75V special-shaped steel rails obtained by this method meet the following requirements: tensile strength Rm ≥ 1160MPa in the forming section, elongation after fracture A ≥ 11.5%; and the hardness of the rail top surface in the forming section, transition section, and heat-affected zone is between 280-330HB.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of rail production technology, specifically relating to a method for producing 60-50kg / m U75V special-shaped rails that do not require normalizing heat treatment. Background Technology

[0002] Currently, most domestic heavy-haul lines, mixed passenger and freight lines, freight lines, intercity lines, and urban subways use symmetrical rails with cross-sections of 50kg / m, 60kg / m, or 75kg / m within the standard range. With the rapid development of China's railways, more and more lines are under construction and will eventually connect to regional or national railway networks, forming a vast and developed domestic railway transportation network. Due to differences in transportation conditions, service environments, and train axle loads between existing lines and newly built lines, and considering the economic efficiency of rail laying, different rail types are used for different lines, roughly categorized as 50kg / m rail lines, 60kg / m rail lines, and 75kg / m rail lines. Lines with different cross-section rails require the use of forged special-shaped rails for connection. The forged special-shaped rail connection method has advantages such as safety and reliability, good mechanical properties, excellent structure, high utilization rate, and high cost-effectiveness, ensuring safe and stable train operation across lines with different cross-section rails.

[0003] Traditionally produced 60-50kg / m U75V special-shaped rails, after high-temperature die forging, have a coarse lamellar pearlite microstructure. To restore the performance of the forged area at the rail heel end, it is necessary to re-normalize the forged area. For example, patent application number 201310431374.4 discloses a heat treatment device and method for the formed rail heel end section. This patent mainly involves a heat treatment device for the formed rail heel end section, but does not describe the heat treatment process or method for the formed rail heel end section. Patent document with application number 201910277768.6 discloses a heat treatment method for the forged section of rail heel. After heating the rail heel forging section to 850-950℃, the rail head is cooled by air jet to 350-500℃. The rail head air jet cooling temperature of this patent is between 350-500℃. The excessively low cooling temperature leads to abnormal rail structure and excessive hardness of the formed section of the rail. Moreover, the wide cooling range is not suitable for the promotion and application of the patent. The document "60AT1-U75V Rail Heel End Induction Heat Treatment" discusses the online heat treatment of 60AT1-U75V rails, which uses medium-frequency induction preheating + medium-frequency induction heating + air jet cooling + spray cooling for the heel end. The performance requirements of this document are different from those of the 60-50kg / m U75V hot-rolled rail standard of this invention, and the process is not universal. Moreover, the medium-frequency induction preheating and spray cooling process described in this document increases the production process, production cost and control difficulty of special-shaped rails, and the spray cooling treatment of the rail head is very likely to cause abnormal structure during continuous production. Summary of the Invention

[0004] To address the problems existing in the prior art, one aspect of the present invention provides a method for producing 60-50kg / m U75V special-shaped steel rails without normalizing heat treatment, comprising the following process flow: blanking → forging → shot blasting → straightening → milling → fine adjustment → length setting → drilling → flaw detection → finished product. Instead of traditional normalizing heat treatment after the forging process, the residual heat of the rail during forging is used to perform controlled cooling treatment on the forming section, transition section, and heat-affected zone of the special-shaped steel rail, including:

[0005] 1) The heel end of the 60kg / m U75V steel rail is forged into a 50kg / m steel rail through two high-temperature die forgings to form a 60-50kg / m U75V special-shaped steel rail; the heating temperature of the first forging is controlled at 880-920℃, and the heating temperature of the second forging is controlled at 1080-1120℃.

[0006] 2) After the secondary forging of 60-50kg / m U75V special-shaped steel rails, the high-temperature, forged rails are immediately placed on a spray cooling device. The forming section, transition section, and heat-affected zone of the special-shaped rails are treated separately with spray cooling. The main focus is on controlling the cooling of the top and sides of the rail head, with the spray cooling area covering at least 50mm of the forging heat-affected zone.

[0007] Cooling process for the forming section: The air pressure on the top surface of the rail head is 0.10-0.15MPa, and the cooling rate is 2.0-3.0℃ / s. The air pressure on the side of the rail head is 0.10-0.15MPa, and the cooling rate is 1.5-2.5℃ / s. The forming section of the rail head is cooled from 1000±10℃ to 550±10℃, and the return temperature is controlled at 580±20℃.

[0008] Transition section cooling process: The air pressure on the top surface of the rail head is 0.12-0.16MPa, and the cooling rate is 2.5-3.5℃ / s. The air pressure on the side of the rail head is 0.13-0.18MPa, and the cooling rate is 2.0-3.0℃ / s. The rail head of the transition section is cooled from 1000±10℃ to 530±10℃, and the return temperature is controlled at 560±20℃.

[0009] Cooling process for the heat-affected zone: The air pressure on the top surface of the rail head is 0.15-0.20MPa, and the cooling rate is 3.0-5.0℃ / s. The air pressure on the side surface of the rail head is 0.15-0.20MPa, and the cooling rate is 2.5-4.0℃ / s. The rail head in the heat-affected zone is cooled from 930±10℃ to 500±10℃, and the return temperature is controlled at 540±20℃.

[0010] 3) After the special-shaped steel rails reach the target temperature by controlling the cooling at different positions, they are air-cooled to room temperature.

[0011] In some embodiments, the chemical composition of the 60-50kg / m U75V special-shaped steel rail, by weight percentage, is C: 0.71-0.80%, Si: 0.50-0.80%, Mn: 0.75-1.05%, V: 0.04-0.12%, P≤0.025%, S≤0.025%, Al: ≤0.010%, with the remainder being Fe and unavoidable impurities.

[0012] In some implementations, the mechanical properties of the obtained 60-50kg / m U75V special-shaped rails meet the following requirements: tensile strength Rm of the formed section ≥ 1160MPa, elongation after fracture A ≥ 11.5%; and the hardness of the rail top surface of the formed section, transition section and heat-affected zone is between 280-330HB.

[0013] In some implementations, the forming section and transition section of the obtained 60-50kg / m U75V special-shaped rail are typical pearlitic with a small amount of ferrite structure, without harmful structures such as high-carbon martensite and Widmanstätten, and no overheating phenomenon is observed in the forming section and transition section of the rail.

[0014] In some implementations, the decarburized layer depth of the rail head in the transition section of the 60-50kg / m U75V special-shaped rail is ≤0.21mm.

[0015] Another aspect of the present invention provides a 60-50kg / m U75V special-shaped steel rail, which is obtained by the above-described production method.

[0016] The advantages of this invention are as follows: After the special-shaped rail is forged, it does not undergo the traditional normalizing heat treatment step. Instead, it directly utilizes the residual heat of the rail during the forging process to immediately perform separate air spray treatment on the forming section, transition section, and heat-affected zone of the special-shaped rail. The focus is on the air spray control cooling treatment on the top surface and side surface of the rail head, thereby achieving the purpose of improving the strength, hardness, and refining the microstructure of the rail. Compared with the traditional special-shaped rail production process (material cutting → forging → normalizing heat treatment → shot blasting → straightening → milling → fine adjustment → length setting → drilling → flaw detection → finished product), the normalizing heat treatment step is omitted, simplifying the production process. Furthermore, the mechanical properties of the obtained 60-50kg / m U75V special-shaped rails meet the following requirements: tensile strength Rm≥1160MPa in the forming section, elongation after fracture A≥11.5%; the hardness of the rail top surface in the forming section, transition section, and heat-affected zone is between 280-330HB, with no high or low points exceeding the hardness standard, and the hardness of the entire special-shaped rail is uniform and meets the standard requirements; the microstructure of the forming section and transition section is consistent with the type of the base material, with no abnormal structure, no overheating phenomenon, and the decarburization layer depth of the transition section is ≤0.21mm. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the hardness test of the top surface of the heel-end forming steel rail.

[0018] Figure 2 The hardness test results are for the top surface of the steel rail produced in Example 1.

[0019] Figure 3 The hardness test results are for the top surface of the steel rail produced in Example 2.

[0020] Figure 4 The hardness test results are for the top surface of the rail produced in Example 3.

[0021] Figure 5 The microstructure of the forming section (a), transition section (b), and base material (c) of the irregular-shaped rail in Example 3 is shown.

[0022] Figure 6The microstructure of the decarburized layer in the transition section of the irregular-shaped rail in Example 3. Detailed Implementation

[0023] The present invention will be described in detail below through specific embodiments. These embodiments are intended to help understand the present invention and are not intended to limit the scope of the present invention.

[0024] The traditional manufacturing process for 60-50kg / m U75V special-shaped steel rails is as follows:

[0025] Material cutting → forging → normalizing heat treatment → shot blasting → straightening → milling → fine adjustment → length setting → drilling → flaw detection → finished product. After forging, the irregular-shaped rails are air-cooled to room temperature, and then re-normalized and cooled to refine the microstructure and increase hardness. This invention omits the normalizing heat treatment step. After forging, the residual heat from the rail is used to immediately spray air onto the forming section, transition section, and heat-affected zone of the irregular-shaped rail, focusing on controlled cooling of the top and sides of the rail head, thereby improving the rail's strength, hardness, and refining its microstructure.

[0026] The specific implementation method is as follows:

[0027] 1) The 60-50kg / m U75V special-shaped steel rails used for forging are mainly reinforced by C, Si, Mn and V. The weight percentage of the chemical composition of the rails is C: 0.71-0.80%, Si: 0.50-0.80%, Mn: 0.75-1.05%, V: 0.04-0.12%, P≤0.025%, S≤0.025%, Al: ≤0.010%, and the remainder is Fe.

[0028] 2) The above-mentioned 60kg / m U75V steel rails are forged twice at high temperature to form 50kg / m steel rails, forming 60-50kg / m U75V special-shaped steel rails. The heating temperature of the first forging is controlled at around 900℃ (e.g., 880-920℃), and the heating temperature of the second forging is controlled at around 1100℃ (e.g., 1080-1120℃).

[0029] 3) After the second forging of 60-50kg / m U75V special-shaped steel rails, immediately place the high-temperature, forged rails into a spray cooling device. The forming section, transition section, and heat-affected zone of the special-shaped rails are treated separately with spray cooling. Controlled air cooling is applied to the top and sides of the rail head, while air cooling is applied to the rail web and bottom. The air cooling area covers the forging heat-affected zone by more than 50mm.

[0030] Cooling process for the forming section: The air pressure on the top surface of the rail head is 0.10-0.15MPa, and the cooling rate is 2.0-3.0℃ / s. The air pressure on the side of the rail head is 0.10-0.15MPa, and the cooling rate is 1.5-2.5℃ / s. The forming section of the rail head is cooled from 1000±10℃ to 550±10℃, and the return temperature is controlled at 580±20℃.

[0031] Transition section cooling process: The air pressure on the top surface of the rail head is 0.12-0.16MPa, and the cooling rate is 2.5-3.5℃ / s. The air pressure on the side of the rail head is 0.13-0.18MPa, and the cooling rate is 2.0-3.0℃ / s. The rail head of the transition section is cooled from 1000±10℃ to 530±10℃, and the return temperature is controlled at 560±20℃.

[0032] Cooling process for the heat-affected zone: The air pressure on the top surface of the rail head is 0.15-0.20MPa, and the cooling rate is 3.0-5.0℃ / s. The air pressure on the side surface of the rail head is 0.15-0.20MPa, and the cooling rate is 2.5-4.0℃ / s. The rail head in the heat-affected zone is cooled from 930±10℃ to 500±10℃, and the return temperature is controlled at 540±20℃.

[0033] 4) After the special-shaped rail forming section, transition section and heat-affected zone reach the target temperature through controlled cooling, air cool to room temperature.

[0034] During implementation, the focus was on the forging area at the heel end of irregularly shaped rails. A comparative analysis of the rail head surface hardness at different locations and with different heat treatment processes was conducted to determine the optimal heat treatment process. The results of hardness testing of the rail head surface during the implementation process are also provided. Figure 1 .

[0035] During the implementation process, the main adjustment parameters for the heat treatment process of the forging area at the heel end of the irregularly shaped rail are shown in Table 1.

[0036] Table 1 Comparison of different heat treatment processes during implementation.

[0037]

[0038] As shown in Table 1, after the rail in Example 1 was forged, the special-shaped rail was reheated to 1000-1020℃ and then subjected to controlled cooling treatment. In Examples 2 and 3, the residual heat of the rail during the forging process was used for controlled cooling treatment, and the re-normalizing heat treatment step was omitted. Example 2 used the same final cooling temperature and cooling rate, while Example 3 used different heat treatment processes for different positions of the special-shaped rail.

[0039] The Brinell hardness test of the rail head top surface was conducted according to "TB / T2344.3-2018 Steel Rails Part 3: Special-shaped Steel Rails". The top surface of the rail head was ground down by 0.5 mm or more. The measuring points were spaced 100 mm apart in the forming and transition sections; for the special-shaped portion extending from the base material, the measuring points were spaced 10 mm apart. The rail head surface hardness test results for Examples 1-3 are shown in [reference needed]. Figures 2-4 .

[0040] Depend on Figure 2 It can be seen that the hardness of the top surface of the irregular-shaped rail forming section, transition section, and heat-affected zone (including zone S) in Example 1 meets the standard requirements. Among them, the hardness of the forming section is close to the upper limit of the hardness of the base material, and the hardness of the heat-affected zone (including zone S) is lower than 280 HBW at 3 measuring points. The hardness difference between the irregular-shaped rail forming section and the heat-affected zone is large, which may lead to "saddle-shaped" wear or corrugation during the service of the rail, and affect the smoothness of the track.

[0041] Depend on Figure 3 It can be seen that the hardness of the top surface of the forming section and transition section of the rail in Example 2 meets the standard requirements, but the hardness is close to the lower limit of the base material hardness, and the hardness of the heat-affected zone (including the S zone) is lower than 280 HBW at 12 measuring points, which does not meet the standard requirement that a maximum of 5 measuring points can have a hardness lower than 280 HBW. The rail in Example 2 is in a forged state, and the high final cooling temperature and low cooling rate cannot improve the hardness of the forming section, transition section and heat-affected zone.

[0042] Depend on Figure 4 It can be seen that the surface hardness of the top surface of the forming section and transition section of the special-shaped rail in Example 3 is between 295-305 HBW, which meets the standard requirement of hardness between 280-330 HBW and matches the hardness of the base material. Only one measuring point in the heat-affected zone (including the S-zone) has a hardness below 280 HBW, meeting the standard requirement of a maximum of five measuring points with hardness below 280 HBW. In Example 3, the rail is in a forged state. Utilizing the residual heat from the forging process, the final cooling temperature and cooling rate of the forming section, transition section, and heat-affected zone of the special-shaped rail are controlled respectively. While meeting the strength and hardness requirements of the special-shaped rail, the normalizing heat treatment step of the forging area during production is omitted.

[0043] According to the test methods in TB / T2344.3-2018 Steel Rails Part 3: Special-shaped Steel Rails, the rail head tensile properties and microstructure of the special-shaped steel rail in Example 3 were analyzed. The tensile properties of the formed section are shown in Table 2, and the microstructures of the formed section, transition section, and base material are shown in Table 3. Figure 5 .

[0044] Table 2 Tensile properties of rail forming section in Example 3

[0045]

[0046] From Table 2 and Figure 5It can be seen that the tensile strength Rm of the formed section of the special-shaped rail in Example 3 is ≥1162MPa and the elongation after fracture A is ≥11.5%, which meets the standard requirements. The formed section and transition section of the special-shaped rail in Example 3 are typical pearlitic structures with a small amount of ferrite, which are consistent with the type of the base material. There are no harmful structures such as high-carbon martensite and Widmanstätten, and no overheating phenomenon was observed in the formed section and transition section of the rail.

[0047] Example 3: Decarburized layer sample from the rail head of an irregularly shaped rail. The microstructure of the decarburized layer is shown in the image below. Figure 6 As shown, the decarburization layer depth of the rail head in the transition section is approximately 0.21 mm, which meets the standard requirement of a decarburization layer depth ≤ 0.50 mm.

[0048] This invention addresses the production process of 60-50kg / m U75V special-shaped steel rails by utilizing the residual heat from the forging process to separately spray air onto the forming section, transition section, and heat-affected zone of the special-shaped steel rail. The final cooling temperature and cooling rate at different locations are controlled separately, thereby improving the strength, hardness, and microstructure of the steel rail. While meeting standard requirements, compared to traditional special-shaped steel rail production processes, this invention omits the normalizing heat treatment step in the forging area, simplifying the production process, improving work efficiency, reducing energy consumption and labor costs, and effectively increasing the profit margin of special-shaped steel rail production.

[0049] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for producing 60-50kg / m U75V special-shaped steel rails without normalizing heat treatment, characterized in that, The production method includes the following process flow: blanking → forging → shot blasting → straightening → milling → fine adjustment → length setting → drilling → flaw detection → finished product. Instead of traditional normalizing heat treatment after the forging process, the residual heat from the forging process is used to control the cooling of the forming section, transition section, and heat-affected zone of the special-shaped rail, including: 1) The heel end of the 60kg / m U75V steel rail is forged into a 50kg / m steel rail twice at high temperature to form a 60-50kg / m U75V special-shaped steel rail; the heating temperature of the first forging is controlled at 880-920℃, and the heating temperature of the second forging is controlled at 1080-1120℃. 2) After the secondary forging of 60-50kg / m U75V special-shaped steel rails, the high-temperature, forged rails are immediately placed on a spray cooling device. The forming section, transition section, and heat-affected zone of the special-shaped rails are treated with separate spray cooling. Controlled cooling is applied to the top and sides of the rail head, with the spray cooling area covering at least 50mm of the forging heat-affected zone. Cooling process for the forming section: The air pressure on the top surface of the rail head is 0.10-0.15MPa, and the cooling rate is 2.0-3.0℃ / s. The air pressure on the side of the rail head is 0.10-0.15MPa, and the cooling rate is 1.5-2.5℃ / s. The forming section of the rail head is cooled from 1000±10℃ to 550±10℃, and the return temperature is controlled at 580±20℃. Transition section cooling process: The air pressure on the top surface of the rail head is 0.12-0.16MPa, and the cooling rate is 2.5-3.5℃ / s. The air pressure on the side of the rail head is 0.13-0.18MPa, and the cooling rate is 2.0-3.0℃ / s. The rail head of the transition section is cooled from 1000±10℃ to 530±10℃, and the return temperature is controlled at 560±20℃. Cooling process for the heat-affected zone: The air pressure on the top surface of the rail head is 0.15-0.20MPa, and the cooling rate is 3.0-5.0℃ / s. The air pressure on the side surface of the rail head is 0.15-0.20MPa, and the cooling rate is 2.5-4.0℃ / s. The rail head in the heat-affected zone is cooled from 930±10℃ to 500±10℃, and the return temperature is controlled at 540±20℃. 3) After the special-shaped steel rails reach the target temperature through controlled cooling at different locations, they are then air-cooled to room temperature; The chemical composition of the 60-50kg / m U75V special-shaped steel rail, by weight percentage, is C: 0.71-0.80%, Si: 0.50-0.80%, Mn: 0.75-1.05%, V: 0.04-0.12%, P≤0.025%, S≤0.025%, Al: ≤0.010%, with the remainder being Fe and unavoidable impurities; The mechanical properties of the obtained 60-50kg / m U75V special-shaped rails meet the following requirements: tensile strength Rm of the formed section ≥ 1160MPa, elongation after fracture A ≥ 11.5%; hardness of the rail top surface of the formed section, transition section and heat-affected zone is between 280-330HB; and the decarburization layer depth of the rail head of the transition section of the obtained 60-50kg / m U75V special-shaped rails is ≤ 0.21mm. The formed section and transition section of the obtained 60-50kg / m U75V special-shaped rail are typical pearlitic with a small amount of ferrite structure, without harmful structures such as high-carbon martensite and Widmanstätten, and no overheating phenomenon was observed in the formed section and transition section of the rail.

2. A 60-50kg / m U75V special-shaped steel rail, which is obtained by the production method described in claim 1.

Citation Information

Patent Citations

  • Heat treatment method and heat treatment method for steel rail profiling heel end section

    CN103540736B

  • Thermal treatment method of steel rail heel forging section

    CN110042210A