Preparation method of early-strength high interfacial bonding performance repairing material for solid waste disposal
By laying aggregate and wire mesh on the concrete surface to form a conductive path, and then energizing it to prepare a self-heating repair material, the problem of weak interface of tailings solid waste in concrete is solved. This achieves high performance and early strength at high dosage, and improves the interfacial bonding performance and overall mechanical properties.
Patent Information
- Application Number
- CN202410170493.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-06
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-02-06
AI Technical Summary
When tailings solid waste is efficiently utilized in concrete, there is a problem of a weak interface transition zone, which leads to poor mechanical properties of the concrete. In particular, under high admixture conditions, the weak layer in the interface transition zone cracks first, penetrating the weak zone and affecting the overall performance.
By laying aggregates on the surface to be repaired and inserting metal wire mesh, the aggregates overlap to form a conductive path, and then electrifying the surface to prepare a self-heating repair material. Combined with the pouring and curing of cement slurry, the temperature is controlled between 30℃ and 90℃ to achieve early strength and high interfacial bonding performance.
It achieves high-value utilization of high-dosage solid waste, rapidly improves interfacial bonding strength, repairs the density of the interfacial area, enhances the overall performance of the repair material, resolves the contradiction between dosage and performance, and achieves early strength without affecting later shrinkage or creep.
Smart Images

Figure CN118084422B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of concrete repair, and in particular relates to a method for preparing a repair material with early strength and high interfacial bonding performance for disposing of solid waste. Background Technology
[0002] The statements in this section are merely background information related to the present invention and do not necessarily constitute prior art.
[0003] Tailings solid waste is a major type of industrial solid waste. Open-air dumping of tailings wastes a significant amount of land resources and poses safety hazards to the ecological environment and surrounding residents. One feasible way to utilize tailings solid waste in green building materials is as aggregate to replace traditional sand and gravel in the preparation of infrastructure repair materials to extend their lifespan. However, the efficient resource utilization of solid waste faces a contradiction between dosage and performance. The core issue is that excessive dosage creates an interface transition zone that restricts macroscopic performance. Excessive dosage also results in multiple weak layers in the interface transition zone. During concrete stress, the internal weak layers crack first, and the cracks then penetrate the weak zone, leading to poor mechanical properties of the concrete. When using tailings solid waste to prepare repair materials for the repair of existing concrete, the same interface transition zone exists, and the weakness of this transition zone restricts the utilization efficiency of tailings solid waste. Summary of the Invention
[0004] In order to solve the technical problems existing in the background art, the present invention provides a method for preparing a repair material with early strength and high interfacial bonding performance for disposing of solid waste, which can realize high-value utilization of conductive tailings solid waste.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] The present invention provides a method for preparing a first type of early-strength, high-interfacial-adhesion remediation material for solid waste disposal, comprising:
[0007] According to the preset conductive path, at least two overlapping layers of aggregate are laid on the surface to be repaired.
[0008] In the laid aggregate, pairs of wire mesh are inserted perpendicularly to the surface to be repaired;
[0009] The cement grout is poured from bottom to top until it covers the aggregate.
[0010] By electrifying the metal wire mesh and utilizing the conductive path formed by the overlapping aggregates, a self-heating repair material can be prepared.
[0011] Furthermore, during the process of pouring cement grout from bottom to top, grout is injected sequentially from bottom to top through grouting pipes. As the grouting process progresses, the grouting pipes are continuously pulled upwards until the grouting is completed.
[0012] Furthermore, the curing temperature of the repair materials is controlled between 30℃ and 90℃.
[0013] Furthermore, the repair material begins curing upon completion of pouring, with a curing cycle of 1-3 days and a curing temperature that is uniformly increased from 20℃ at a rate of 0.5℃-2℃ per hour.
[0014] The present invention provides a method for preparing a second type of early-strength, high-interfacial-adhesion remediation material for solid waste disposal, comprising:
[0015] Insert a pair of metal wire mesh sheets perpendicular to the surface to be repaired;
[0016] A single layer of aggregate is laid on the surface to be repaired, with contact between adjacent aggregates;
[0017] The cement grout is poured onto the surface of the aggregate in a predetermined path so that the cement grout sinks into the gaps between the aggregates.
[0018] Then lay the second layer of aggregate, with contact between adjacent aggregates. Pour cement grout into the gaps between the aggregates, and repeat this process until the set repair height is achieved.
[0019] By electrifying the metal wire mesh and utilizing the conductive path formed by the overlapping aggregates, a self-heating repair material can be prepared.
[0020] Furthermore, the cement slurry is poured onto the aggregate surface in a "1" or "S" shaped path.
[0021] Furthermore, the curing temperature of the repair materials is controlled between 30℃ and 90℃.
[0022] Furthermore, the repair material begins curing upon completion of pouring, with a curing cycle of 1-3 days and a curing temperature that is uniformly increased from 20℃ at a rate of 0.5℃-2℃ per hour.
[0023] The present invention provides a method for preparing a third type of early-strength, high-interfacial-adhesion remediation material for solid waste disposal, comprising:
[0024] Conductive fibers are added to a cement grout containing aggregate and then poured onto the surface to be repaired.
[0025] Insert a pair of metal wire mesh sheets perpendicular to the surface to be repaired;
[0026] By electrifying the metal wire mesh, a self-heating repair material is prepared by utilizing the conductive path formed by the overlap of aggregates and conductive fibers.
[0027] Furthermore, the repair material begins curing upon completion of pouring, with the curing temperature controlled between 30℃ and 90℃, and the curing cycle lasting 1-3 days. The curing temperature is increased uniformly from 20℃ at a rate of 0.5℃-2℃ per hour.
[0028] The beneficial effects of this invention are:
[0029] (1) This invention solves the contradiction between dosage and performance, and provides a new method for the efficient utilization of bulk solid waste, especially the utilization of conductive mineral bulk solid waste, such as copper tailings and iron tailings, to achieve high-value utilization of conductive tailings solid waste, that is, high dosage and high performance are developed simultaneously, that is, concrete does not have reduced mechanical properties when the dosage of tailings solid waste is high.
[0030] (2) The ordinary silicate cement-based repair material prepared by the present invention without adding early strength agent achieves early strength function, rapidly improves the interfacial bonding strength in a short period of time, utilizes the conductive properties of solid waste aggregate to form a current path by overlapping each other, and realizes the function of heating and curing by inputting current. The repair material system does not contain early strength agent components and will not affect the later shrinkage or creep of the repair material.
[0031] (3) The method of the present invention achieves the dual functions of regulating and repairing the interface transition zone and the aggregate interface transition zone, playing a dual role of consuming a large amount of raw materials and enhancing the repair application function, thus seeking a new path for the efficient utilization of solid waste; under the electrothermal curing, the degree of cement hydration around the aggregate in the tailings aggregate interface transition zone is improved, and the interface zone is dense. As an integral repair material, the electrothermal curing increases the hydration process of the repair material, and the repair interface zone is dense, thus playing a dual role.
[0032] Advantages of additional aspects of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0033] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0034] Figure 1 This is a schematic diagram of preparation scheme 1 of the early-strength, high-interfacial-adhesion repair material for solid waste disposal according to the present invention;
[0035] Figure 2 This is a schematic diagram of preparation scheme 2 of the early-strength, high-interfacial-adhesion repair material for solid waste disposal according to the present invention;
[0036] Figure 3 This is a schematic diagram of preparation scheme 3 of the early-strength, high-interfacial-adhesion repair material for solid waste disposal according to the present invention. Detailed Implementation
[0037] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0038] It should be noted that the following detailed description is illustrative and intended to provide further explanation of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0039] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.
[0040] Figure 1 This is a schematic diagram of preparation scheme 1 of the early-strength, high-interfacial-adhesion remediation material for solid waste disposal according to the present invention. The scheme includes:
[0041] Step a1: According to the preset conductive path, lay at least two overlapping layers of aggregate on the surface to be repaired.
[0042] Before implementing step a1, the following is also included:
[0043] Roughen the concrete substrate surface to be repaired and clean it thoroughly.
[0044] Step a2: Insert pairs of wire mesh perpendicular to the surface to be repaired into the laid aggregate.
[0045] For example, the wire mesh should protrude 5-12cm above the repair material, and the mesh spacing should be 5-10mm on each side. The distance between two wire mesh panels should be greater than 10cm and less than 50cm.
[0046] It should be noted that the material and size of the wire mesh can be set by those skilled in the art according to the actual situation, and will not be described in detail here.
[0047] Step a3: Pour the cement grout from bottom to top until it covers the aggregate. The flowability of the cement grout should be no less than 300 mm.
[0048] Specifically, during the process of pouring cement grout from bottom to top, grout is injected sequentially from bottom to top through grouting pipes. As the grouting process progresses, the grouting pipes are continuously pulled upwards until the grouting is completed.
[0049] Step a4: By passing an electric current through the metal wire mesh, a self-heating repair material is prepared by utilizing the conductive path formed by the overlapping of the aggregates.
[0050] In this embodiment, aggregates are pre-laid and then the grout is poured. Since the aggregates are not mixed beforehand and their surfaces are not coated with cement grout, there is contact between the aggregates, which makes it possible to pass current through them and create a closed current loop. The current flow path can be optimized through the aggregate gradation design.
[0051] To prevent the repair material from expanding due to temperature rise, which could damage the microstructure of the repair interface and pose a potential threat to the repair interface, the curing temperature is controlled between 30℃ and 90℃. The curing temperature is achieved by controlling the voltage, which is controlled within the range of 100V-220V. Power is cut off after the curing temperature is reached, and power is automatically turned on when the temperature is lower than the design temperature to continue heating. The repair material is poured and curing begins. The curing cycle is 1-3 days, and the curing temperature is increased uniformly from 20℃ at a rate of 0.5℃-2℃ per hour.
[0052] The repair material consists of: 320-580 parts cement, 120-200 parts water, 0-300 parts sand, 1300-1900 parts aggregate, and 7-15 parts water-reducing agent. The repair material can be made of ordinary concrete or ultra-high performance concrete, not limited to the above-mentioned concrete component ratios. Because the aggregate is deposited on the repair surface before being filled with grout, this repair method does not require a monolithic repair, thus accommodating a higher amount of aggregate compared to repair materials formed by mixing aggregate and cement.
[0053] Characteristics of the repair materials: The cement is ordinary silicate cement, the water is deionized water, the sand is fine particles of conductive ore with a particle size of less than 3mm, the aggregate is conductive ore particles with a particle size of 10mm-15mm, such as iron tailings and copper tailings, and the water-reducing agent is polycarboxylate water-reducing agent.
[0054] During the preparation of the repair material, cement and sand are mixed and stirred for 3-5 minutes, and water and water-reducing agent are added and stirred for 4-8 minutes.
[0055] Figure 2 This is a schematic diagram of preparation scheme 2 of the early-strength, high-interfacial-adhesion remediation material for solid waste disposal according to the present invention. The scheme includes:
[0056] Step b1: Insert a pair of wire mesh sheets perpendicular to the surface to be repaired.
[0057] Before implementing step b1, the following is also included:
[0058] Roughen the concrete substrate surface to be repaired and clean it thoroughly.
[0059] For example, the wire mesh should protrude 5-12cm above the repair material, and the mesh spacing should be 5-10mm on each side. The distance between two wire mesh panels should be greater than 10cm and less than 50cm.
[0060] It should be noted that the material and size of the wire mesh can be set by those skilled in the art according to the actual situation, and will not be described in detail here.
[0061] Step b2: Lay a single layer of aggregate on the surface to be repaired, with contact between adjacent aggregates.
[0062] In this process, cement slurry is poured onto the surface of the aggregate in a “1” or “S” shape.
[0063] It is understood here that those skilled in the art may also use other slurry dumping routes, with the dumping route designed to allow the slurry to sink into the gaps between the aggregates under the action of gravity.
[0064] Step b3: Pour the cement grout onto the aggregate surface along a predetermined path, allowing the cement grout to sink into the gaps between the aggregates. The flowability of the cement grout should be no less than 280 mm.
[0065] Step b4: Lay the second layer of aggregate, with contact between adjacent aggregates. Pour cement grout into the gaps between the aggregates, and repeat this process until the set repair height is achieved.
[0066] Step b5: Apply electricity to the metal wire mesh and use the conductive path formed by the overlapping of the aggregates to prepare a self-heating repair material.
[0067] This scheme is a sandwich design based on aggregate and cement paste. The aggregate layer is the layer through which current passes efficiently, and the hydration products of the cement paste layer provide the overall mechanical properties of the repair material. The mechanical strength is improved by the heat radiation generated by the aggregate to the cement paste layer. Scheme 2 uses a single layer of aggregate, but it is necessary to ensure close contact between the aggregates in the single layer to increase the possibility of conductive paths. The cement paste sinks into the gaps between the single-layer aggregates, and the flowability of the cement paste is lower than that of the cement paste in Scheme 1, which sinks into the gaps between multiple layers of aggregates. The conductive paths in the sandwich design can be achieved by laying single layers of aggregate and designing the particle gradation to achieve a high contact area between the aggregates.
[0068] To prevent the expansion of the repair material caused by temperature rise, which could damage the microstructure of the repair interface and pose a potential threat to the repair interface, the curing temperature is controlled between 30℃ and 90℃. The curing temperature is achieved by controlling the voltage, with a control range of 100V-220V. Power is cut off after the curing temperature is reached, and power is automatically turned on when the temperature is lower than the design temperature to continue heating. The repair material is poured and curing begins, with a curing cycle of 1-3 days. The curing temperature is uniformly increased from 20℃ at a rate of 0.5℃-2℃ per hour. Because the aggregate in Pathway 2 is laid in a single layer to form a pathway, the slurry cannot form a conductive pathway. Therefore, Pathway 2 achieves the same repair effect as Pathway 1, but the power input is 20%-40% higher and the amount of slurry repair material used is 15%-30% higher.
[0069] Repair material composition: 420-690 parts cement, 140-280 parts water, 0-400 parts sand, 1000-1600 parts aggregate, and 8-17 parts water-reducing agent.
[0070] It should be noted that the repair material composition can be ordinary concrete or ultra-high performance concrete, and is not limited to the above concrete component ratio.
[0071] Repair material characteristics: The cement is ordinary silicate cement, the water is deionized water, the sand is fine particles of conductive ore, for example, with a particle size of less than 3 mm, the aggregate is conductive ore particles with a particle size of 10 mm-15 mm, such as iron tailings and copper tailings, and the water-reducing agent is polycarboxylate water-reducing agent.
[0072] During the preparation of the repair material, cement and sand are mixed and stirred for 3-5 minutes, and water and water-reducing agent are added and stirred for 4-8 minutes.
[0073] Figure 3 This is a schematic diagram of preparation scheme 3 of the early-strength, high-interfacial-adhesion remediation material for solid waste disposal according to the present invention. The scheme includes:
[0074] Step c1: Add conductive fibers to the cement slurry containing aggregate and pour it onto the surface to be repaired;
[0075] Step c2: Insert a pair of metal wire mesh sheets perpendicular to the surface to be repaired;
[0076] Step c3: Electricity is applied to the metal wire mesh, and a self-heating repair material is prepared by utilizing the conductive path formed by the overlap of aggregates and conductive fibers.
[0077] For example, the wire mesh should protrude 5-12cm above the repair material, and the mesh spacing should be 5-10mm on each side. The distance between two wire mesh panels should be greater than 10cm and less than 50cm.
[0078] It should be noted that the material and size of the wire mesh can be set by those skilled in the art according to the actual situation, and will not be described in detail here.
[0079] In this repair scheme, the aggregate-cement slurry is mixed. The mixture itself is fluid. During the repair, there is no cement slurry settling into the gaps between the aggregates. Therefore, the fluidity of the mixture only needs to meet the requirements of workability. However, in this scheme, the surface of the aggregate is covered by cement slurry, and the connectivity of the aggregate in the mixture is cut off by the cement slurry. In order to achieve high efficiency of the conductive path, it is necessary to introduce conductive fibers into the slurry to overlap the non-contact aggregates that are cut off by the cement slurry.
[0080] To prevent the repair material from expanding due to temperature rise, which could damage the microstructure of the repair interface and pose a potential threat to the repair interface, the curing temperature is controlled between 30℃ and 90℃. This curing temperature is achieved by controlling the voltage, with a control range of 100V-220V. Power is cut off once the curing temperature is reached, and automatically re-energized when the temperature drops below the design temperature to continue heating. Curing begins after the repair material is poured, with a curing period of 1-3 days. The curing temperature starts at 20℃ and increases uniformly at a rate of 0.5℃-2℃ per hour. Since the concrete in method 3 is mixed, the aggregate surface is coated with cement slurry, affecting direct contact with the aggregate surface. Therefore, conductive fibers need to be placed in the slurry to connect the aggregate and form a conductive path.
[0081] The repair materials in this plan consist of: 450-790 parts cement, 150-320 parts water, 100-500 parts sand, 1000-1300 parts aggregate, 8-17 parts water-reducing agent, and 50-160 parts steel fiber.
[0082] It should be noted that the repair material composition of this solution can be ordinary concrete or ultra-high performance concrete, but unlike solutions one and two, this solution must also contain conductive fibers, which can be steel fibers or carbon fibers.
[0083] The repair materials used in this solution are characterized as follows: the cement is ordinary silicate cement, the water is deionized water, the sand is fine-grained conductive ore with a particle size of less than 3 mm, the aggregate is conductive ore particles with a particle size of 10 mm-15 mm, such as iron tailings or copper tailings, the water-reducing agent is polycarboxylate water-reducing agent, and the steel fiber is copper-plated straight steel fiber with a diameter of 20 μm and a length of 13 mm.
[0084] During the preparation of the repair material, cement, sand and coarse aggregate are mixed and stirred for 3-5 minutes, water and water-reducing agent are added and stirred for 4-8 minutes, and then steel fibers are added and stirred for 5-10 minutes.
[0085] The mechanism of the preparation method of the early-strength, high-interfacial-adhesion remediation material for solid waste disposal of the present invention:
[0086] Aggregates act as conductive media, forming a network of conductive pathways, or aggregates are the primary component supplemented with conductive steel fibers, which interlock to form conductive pathways. Electrothermal curing, with its increased curing temperature, accelerates the reaction kinetics of cement, including faster dissolution, nucleation, and precipitation rates. As the curing temperature rises, the second stage of cement hydration, the tricalcium silicate hydration stage, occurs earlier, approaching the exothermic peak of the first stage, the ettringite formation stage. In the repair material, the cement paste forms a calcium silicate gel outline around the cement particles, with increasing outline thickness and a fibrous gel state. The calcium silicate hydrates form an interconnected network structure, allowing the various components of the cement paste to bind together effectively. This promotes low porosity in the repair material, strengthens the transition zones at the repair and aggregate interfaces, thereby improving both the performance of the repair material and its interfacial bonding properties.
[0087] Example 1:
[0088] The concrete substrate surface to be repaired is roughened by hand and cleaned. Aggregate is laid on the repair surface, and wire mesh is inserted perpendicularly to the surface, extending 10cm above the repair material. The mesh spacing is 6mm on each side, with a 30cm gap between two meshes. Mortar or neat cement paste is mixed to a fluidity of 350mm and injected through a grouting pipe from bottom to top until the grout covers the aggregate. The grouting pipe is continuously pulled upwards during the injection process until grouting is complete.
[0089] By connecting a sinusoidal alternating current to a metal wire mesh and inputting the current, the aggregate overlaps to form an internal conductive path, achieving self-heating of the material. To prevent expansion of the repair material due to temperature rise, which could damage the microstructure of the repair interface and pose a potential threat to the repair interface, the curing temperature is controlled at 50℃. The curing temperature is achieved by controlling the voltage, with a control range of 180V. Power is cut off after the curing temperature is reached, and power is automatically turned on when the temperature drops below the design temperature to continue heating. The repair material self-casts and begins curing. The curing temperature starts at 20℃ and gradually increases to the controlled curing temperature throughout the curing period.
[0090] Example 1: The curing period was 2 days and 3 days, while the control group was cured at standard room temperature for 3 days and 7 days. The repair material consisted of 3240 parts cement, 150 parts water, 150 parts sand, 1700 parts aggregate, and 8 parts water-reducing agent. The bonding performance of the repair interface was tested by pull-out test.
[0091] Results analysis:
[0092] The results from Method 1 show that the interfacial bond strength after 2 days and 3 days of electro-curing is 2.6 MPa and 3.3 MPa, respectively, with the failure mode being concrete matrix failure. In contrast, the interfacial bond strength after 2 days and 3 days of standard curing in the control group is 1.1 MPa and 1.5 MPa, respectively, with the failure mode being interfacial failure. These results demonstrate that this method can achieve better interfacial bond performance for repair under high solid waste content conditions compared to traditional methods.
[0093] Cause analysis: Aggregates, acting as conductive media, form a conductive network. When electricity is applied, the cement-based materials heat up, the curing temperature rises, and the reaction kinetics of cement are accelerated, including faster dissolution, nucleation, and precipitation rates. Calcium silicate hydrates form an interconnected network structure, allowing the various components of the cement stone to bond together better. This promotes the formation of low porosity in the repair material, improves the density of the repair interface and the preferred orientation of calcium hydroxide at the repair interface, and strengthens the transition zone between the repair interface and the aggregate interface. As a result, the performance of the repair material is improved while also enhancing the interfacial bonding performance.
[0094] Table 1 Results of Implementation Method 1
[0095]
[0096]
[0097] Example 3:
[0098] The concrete substrate surface to be repaired is roughened and cleaned. The concrete mixture is poured onto the repair surface, with a flowability of 270 mm. A wire mesh is inserted perpendicular to the repair surface, extending 7 cm above the repair material, with a mesh spacing of 7 mm on each side. The spacing between two wire meshes is 25 cm. The grout is poured onto the aggregate surface in a straight line or other pouring pattern, designed to allow the grout to sink into the aggregate gaps. Under gravity, the grout sinks into the aggregate gaps. A second layer of aggregate is then laid, maintaining contact between the aggregates, and the grout is poured again in a straight line. Under gravity, the grout sinks into the aggregate gaps. This process is repeated until the required repair height is achieved.
[0099] By connecting a sinusoidal alternating current to the metal wire mesh and inputting the current, the aggregate overlaps to form an internal conductive path, achieving self-heating of the material. The curing temperature is controlled at 85℃, achieved by controlling the voltage within a 180V range. Power is cut off once the curing temperature is reached, and automatically re-energized when the temperature drops below the design temperature to continue heating. The repair material self-casts and begins curing, with the curing temperature rising uniformly from 20℃ to the controlled temperature throughout the curing period.
[0100] Example 2: Curing periods of 1 day and 2 days; control group: curing periods of 3 days and 7 days. Repair material composition: 590 parts cement, 200 parts water, 200 parts sand, 1400 parts aggregate, and 12 parts water-reducing agent. Pull-out tests were used to test the bonding performance of the repair interface.
[0101] Results analysis:
[0102] The results from method 3 show that the interfacial bond strength after 1 day and 2 days of electrical curing is 2.6 MPa and 3.1 MPa, respectively, with the failure mode being concrete matrix failure. In contrast, the interfacial bond strength after 3 days and 7 days of standard curing in the control group is 1.4 MPa and 1.7 MPa, respectively, with the failure mode being interfacial failure. These results demonstrate that this method achieves better interfacial bond performance for repair than traditional methods, even with high solid waste content.
[0103] Table 2 Results of Implementation Method 2
[0104] Operating conditions Interfacial adhesion (MPa) Failure Mode Example 2-1d 2.6 Concrete matrix failure Example 2-2d 3.1 Concrete matrix failure control group - 3 days 1.4 Interface failure Control group - 7 days 1.7 Interface failure
[0105] Example 3:
[0106] The concrete substrate surface to be repaired is roughened and cleaned. The concrete mixture is poured onto the surface, with a flowability of 280 mm. A wire mesh is inserted perpendicularly to the surface, extending 8 cm above the repair material, with a mesh spacing of 8 mm on each side. The spacing between two wire meshes is 20 cm. By connecting a sinusoidal alternating current to the wire mesh, the current is applied, and the overlapping aggregate forms an internal conductive path, enabling the material to self-heat.
[0107] To prevent the expansion of the repair material caused by temperature rise, which could damage the microstructure of the repair interface and pose a potential threat to the repair interface, the curing temperature is controlled at 80℃. The curing temperature is achieved by controlling the voltage, with a voltage control range of 180V. Power is cut off after the curing temperature is reached, and power is automatically turned on when the temperature is lower than the design temperature to continue heating. The curing process begins after the repair material is poured, and the curing temperature rises uniformly to the controlled temperature from 20℃ during the curing period.
[0108] Example 3: Curing periods of 1 day and 2 days; curing periods of the control group: 3 days and 7 days. Repair material composition: 560 parts cement, 180 parts water, 300 parts sand, 1200 parts aggregate, 9 parts water-reducing agent, and 80 parts steel fiber. The bonding performance of the repair interface was tested by pull-out tests.
[0109] Results analysis:
[0110] The results from method 3 show that the interfacial bond strength after 1 day and 2 days of electrical curing is 2.4 MPa and 2.9 MPa, respectively, with the failure mode being concrete matrix failure. In contrast, the interfacial bond strength after 3 days and 7 days of standard curing in the control group is 1.2 MPa and 1.6 MPa, respectively, with the failure mode being interfacial failure. These results demonstrate that this method achieves better interfacial bond performance for repairing high-content solid waste compared to traditional methods.
[0111] Cause Analysis: Cement slurry coating the aggregate surface affects direct contact with the aggregate surface. Conductive steel fibers are placed within the slurry to connect the aggregate and form a conductive path. Upon energization, the cement-based material heats up, increasing the curing temperature. The second stage of cement hydration, the tricalcium silicate hydration stage, occurs earlier, approaching the exothermic peak of the first stage, the formation of ettringite. The cement slurry in the repair material forms a calcium silicate gel outline around the cement particles, with increasing outline thickness and a fibrous gel state. The calcium silicate hydrates form an interconnected network structure, allowing the various components of the cement paste to bond well together, strengthening the transition zones at the repair and aggregate interfaces, thereby improving both the performance of the repair material and the interfacial bonding properties.
[0112] Table 3 Results of Implementation Method 3
[0113] Operating conditions Interfacial adhesion (MPa) Failure Mode Example 3-1d 2.4 Concrete matrix failure Example 3-2d 2.9 Concrete matrix failure control group - 3 days 1.2 Interface failure Control group - 7 days 1.6 Interface failure
[0114] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing a remediation material with early strength and high interfacial bonding performance for solid waste disposal, characterized in that, include: According to the preset conductive path, at least two overlapping layers of aggregate are laid on the surface to be repaired. In the laid aggregate, pairs of wire mesh are inserted perpendicularly to the surface to be repaired; The cement grout is poured from bottom to top until it covers the aggregate. By electrifying the metal wire mesh and utilizing the conductive path formed by the overlapping of aggregates, a self-heating repair material can be prepared. Repair material composition: 320-580 parts cement, 120-200 parts water, 0-300 parts sand, 1300-1900 parts aggregate, and 7-15 parts water-reducing agent; The cement is ordinary Portland cement, the water is deionized water, the sand is fine particles of conductive ore with a particle size of less than 3mm, the aggregate is conductive ore particles with a particle size of 10mm-15mm, the conductive ore is iron tailings and copper tailings, and the water-reducing agent is polycarboxylate water-reducing agent. The curing temperature of the repair material is controlled between 30℃ and 90℃, and the voltage is controlled between 100V and 220V. Curing begins as soon as the repair material is poured, with a curing period of 1-3 days. The temperature is increased from 20℃ to the curing control temperature at a rate of 0.5℃-2℃ per hour.
2. The preparation method of the early-strength, high-interfacial-adhesion remediation material for solid waste disposal as described in claim 1, characterized in that, During the process of pouring cement grout from bottom to top, grout is injected sequentially through grouting pipes from bottom to top. As the grouting process progresses, the grouting pipes are continuously pulled upwards until the grouting is completed.
3. A method for preparing a remediation material with early strength and high interfacial bonding performance for solid waste disposal, characterized in that, include: Insert a pair of metal wire mesh sheets perpendicular to the surface to be repaired; A single layer of aggregate is laid on the surface to be repaired, with contact between adjacent aggregates; The cement grout is poured onto the surface of the aggregate in a predetermined path so that the cement grout sinks into the gaps between the aggregates. Then lay the second layer of aggregate, with contact between adjacent aggregates. Pour cement grout into the gaps between the aggregates, and repeat this process until the set repair height is achieved. By electrifying the metal wire mesh and utilizing the conductive path formed by the overlapping of aggregates, a self-heating repair material can be prepared. Repair material composition: 420-690 parts cement, 140-280 parts water, 0-400 parts sand, 1000-1600 parts aggregate, and 8-17 parts water-reducing agent; the cement is ordinary Portland cement, the water is deionized water, the sand is fine particles of conductive ore with a particle size of less than 3mm, the aggregate is conductive ore particles with a particle size of 10mm-15mm, the conductive ore is iron tailings or copper tailings, and the water-reducing agent is polycarboxylate water-reducing agent; The curing temperature of the repair material is controlled between 30℃ and 90℃, and the voltage control range is 100V-220V. Curing begins as soon as the repair material is poured, with a curing period of 1-3 days. The temperature is increased from 20℃ to the curing control temperature at a rate of 0.5℃-2℃ per hour.
4. The preparation method of the early-strength, high-interfacial-adhesion remediation material for solid waste disposal as described in claim 3, characterized in that, The cement grout is shaped like a "1" or... S The material is poured onto the aggregate surface in a "shaped" path.
5. A method for preparing a remediation material with early strength and high interfacial bonding performance for solid waste disposal, characterized in that, include: Add steel fibers to the cement grout containing aggregate and pour it onto the surface to be repaired; Insert a pair of metal wire mesh sheets perpendicular to the surface to be repaired; By electrifying the metal wire mesh, a self-heating repair material is prepared by utilizing the conductive path formed by the overlap of aggregates and conductive fibers. Repair material composition: 450-790 parts cement, 150-320 parts water, 100-500 parts sand, 1000-1300 parts aggregate, 8-17 parts water-reducing agent, and 50-160 parts steel fiber; the cement is ordinary Portland cement, the water is deionized water, the sand is fine particles of conductive ore with a particle size of less than 3mm, the aggregate is conductive ore particles with a particle size of 10mm-15mm, the conductive ore is iron tailings or copper tailings, the water-reducing agent is polycarboxylate water-reducing agent, and the steel fiber is copper-plated straight steel fiber with a diameter of 200μm and a length of 13mm; The curing temperature of the repair material is controlled between 30℃ and 90℃, and the voltage is controlled between 100V and 220V. Curing begins as soon as the repair material is poured, with a curing period of 1-3 days. The temperature is increased from 20℃ to the curing control temperature at a rate of 0.5℃-2℃ per hour.
Citation Information
Patent Citations
Conductive smart modified recycled aggregate concrete and preparation method thereof
CN115819028A