A composite TPE material and preparation method thereof

Through the reaction of SMA with ABS and hollow glass beads, as well as the introduction of EVA, the problem of poor compatibility between ABS resin and rubber powder is solved, and the mechanical properties and compatibility of composite TPE materials are significantly improved.

CN118085509BActive Publication Date: 2024-10-11GUANGDONG KEYUE NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410343165.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-25
Publication Date
2024-10-11
Estimated Expiration
2044-03-25

AI Technical Summary

Technical Problem

When ABS resin and rubber powder are melted and blended, due to poor compatibility, the phase separation phenomenon is serious and the mechanical properties are weakened.

Method used

By reacting the anhydride group in SMA with the hydroxyl group of ABS and hollow glass beads, the free radicals generated by ZDS are used to graft with the PB of ABS, and EVA with both polar and non-polar groups is added. Improve the compatibility and bonding strength of composite materials.

Benefits of technology

It significantly improves the mechanical properties of TPE materials, enhances the compatibility and bonding force between components, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a composite TPE material and a preparation method thereof, and belongs to the technical field of TPE materials. The preparation method thereof comprises: 1) crushing ABS and performing constant temperature treatment to obtain ABS prefabricated material; 2) placing hollow glass microspheres and ABS prefabricated material in sodium hydroxide solution, heating and stirring, and filtering to obtain pretreated material; 3) mixing rubber powder, ZDS and SMA, and then melt blending to obtain material A; 4) mixing SEBS, white oil, PPO, TPEE, EVA, pretreated material, stearic acid, antioxidant and auxiliary agent, adding compatibilizer and stirring evenly, and then melt blending to obtain material B; 5) blending material A and material B to obtain. The present invention significantly improves the compatibility between the components in the TPE composite material through SMA, ABS, hollow glass microspheres, ZDS and EVA, and enhances the bonding force between the materials, thereby greatly improving the mechanical properties of the TPE material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of TPE materials and relates to a composite TPE material and a preparation method thereof. Background Art

[0002] Rubber powder (WTR) is made by grinding the tires of various vehicles after they are replaced through a series of processes, so the source of rubber powder particles is relatively wide. The main particle size of rubber powder commonly used in actual road construction is between 40-80 mesh, and its main components are natural rubber and styrene-butadiene rubber.

[0003] ABS resin is a graft copolymer of three monomers: acrylonitrile, 1,3-butadiene and styrene. In fact, it is often a mixture of a graft copolymer containing butadiene and an acrylonitrile-styrene copolymer, in which acrylonitrile accounts for 15-35%, butadiene accounts for 5-30%, and styrene accounts for 40-60%. However, since acrylonitrile contains polar groups such as cyano, it has poor compatibility with rubber powder. When ABS and rubber powder are melt-blended, severe phase separation will occur, the morphology becomes more complex, and it is usually accompanied by weakened mechanical properties. Summary of the invention

[0004] The object of the present invention is to provide a composite TPE material and a preparation method thereof. The present invention reacts the anhydride groups in SMA, the hydroxyl groups in ABS and hollow glass microspheres, and utilizes the free radical energy generated by ZDS to be grafted with the PB phase of ABS, and adds EVA having both polar groups and non-polar groups, thereby significantly improving the compatibility between the components in the TPE composite material, enhancing the bonding force between the materials, and thus greatly improving the mechanical properties of the TPE material.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a composite TPE material comprises the following steps:

[0007] 1) crushing ABS and subjecting it to constant temperature treatment to obtain ABS prefabricated material;

[0008] 2) placing the hollow glass microspheres and the ABS prefabricated material in a sodium hydroxide solution, heating and stirring, and then filtering to obtain a pretreated material;

[0009] 3) The rubber powder, ZDS and SMA are stirred and mixed, melt-blended, cooled, granulated and dried to obtain material A;

[0010] 4) SEBS, white oil, PPO, TPEE, EVA, pre-treated material, stearic acid, antioxidant and additives are stirred and mixed, a compatibilizer is added, stirred evenly, melt blended, cooled, granulated and dried to obtain material B;

[0011] 5) Material A and material B are blended, extruded, cooled, granulated and dried to obtain a TPE material.

[0012] As a preferred technical solution of the present invention, in step 1), the condition of the constant temperature treatment is at a temperature of 120-130° C. and a constant temperature of 50-60 hours.

[0013] As a preferred technical solution of the present invention, in step 2), the heating and stirring conditions are 75-80°C, 400-700r / min, and stirring for 1.0-1.5h; the concentration of the sodium hydroxide solution is 0.3-0.6moL / L; the mass ratio of the hollow glass microspheres, ABS preform and sodium hydroxide solution is 2.0-2.5:10-12:20-25; the hollow glass microspheres are selected from the group consisting of ABS preforms with a density of 0.12-0.70g / cm 3 , at least one of the particle sizes in the range of 5-100 μm.

[0014] As a preferred technical solution of the present invention, in step 3), the mass ratio of the rubber powder, ZDS and SMA is 10-12:0.6-0.8:1.0-1.5.

[0015] As a preferred technical solution of the present invention, in step 3), the stirring and mixing time is 10-20 minutes; the melt blending condition is carried out at a temperature of 180-190° C.; and the cooling is air cooling to room temperature.

[0016] As a preferred technical solution of the present invention, in step 4), the mass ratio of SEBS, white oil, PPO, TPEE, EVA, pretreated material, stearic acid, antioxidant, additive and compatibilizer is 30:30-35:30-35:90-100:10-16:20-25:5-10:3-5:15-20:10-15.

[0017] As a preferred technical solution of the present invention, in step 4), the auxiliary agent is calcium carbonate, polyethylene wax and polyethylene oxide mixed in a mass ratio of 3.0-3.5:1:1.2-1.5; the antioxidant is one or two of antioxidant 1010 and antioxidant PS802; and the compatibilizer is N,N-diethylformamide.

[0018] As a preferred technical solution of the present invention, in step 4), the stirring and mixing time is 10-20 minutes; the melt blending condition is carried out at a temperature of 190-200°C; and the cooling is air cooling to room temperature.

[0019] As a preferred technical solution of the present invention, in step 5), the mass ratio of material A to material B is 4-5:30-32; the conditions for the co-extrusion are melt extrusion at a temperature of 180-190°C through a twin-screw extruder; and the cooling is cooling to room temperature using circulating water cooling.

[0020] As a preferred technical solution of the present invention, the SMA is a styrene-maleic anhydride copolymer; the ZDS is zinc sorbate; the EVA is an ethylene-vinyl acetate copolymer; PPO is polyphenylene ether; SEBS is a linear triblock copolymer with polystyrene as the terminal segment and ethylene-butylene copolymer obtained by hydrogenating polybutadiene as the middle elastic block, and SEBS does not contain unsaturated double bonds, so it has excellent aging resistance, has both plasticity and high elasticity, and can be processed and used without vulcanization; TPEE is a thermoplastic polyester elastomer, also known as polyester rubber.

[0021] As a preferred technical solution of the present invention, SMA contains non-polar benzene ring groups and polar carboxylic acid groups in its structure, so it shows good compatibility with both hydrophobic materials and hydrophilic materials.

[0022] Beneficial effects of the present invention:

[0023] The present invention reacts the anhydride groups in SMA, the hydroxyl groups in ABS and the hollow glass microspheres, and utilizes the free radical energy generated by ZDS to be grafted with the PB phase of ABS, and adds EVA having both polar groups and non-polar groups, thereby significantly improving the compatibility between the components in the TPE composite material and enhancing the bonding force between the materials, thereby greatly improving the mechanical properties of the TPE material. DETAILED DESCRIPTION

[0024] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0025] Example 1

[0026] A method for preparing a composite TPE material comprises the following steps:

[0027] 1) crushing ABS and subjecting it to constant temperature treatment to obtain ABS prefabricated material; wherein the condition of the constant temperature treatment is at a temperature of 120° C. and a constant temperature of 50 hours;

[0028] 2) placing the hollow glass microspheres and the ABS prefabricated material in a sodium hydroxide solution, heating and stirring, and then filtering to obtain a pretreated material; wherein the heating and stirring conditions are at a temperature of 75° C., a speed of 400 r / min, and stirring for 1.0 h; the concentration of the sodium hydroxide solution is 0.3 mol / L; the mass ratio of the hollow glass microspheres, the ABS prefabricated material and the sodium hydroxide solution is 2.0:10:20; the density of the hollow glass microspheres is 0.50 g / cm 3 , particle size 60 μm;

[0029] 3) The rubber powder, ZDS and SMA are stirred and mixed, melt blended, cooled, granulated and dried to obtain material A; wherein the mass ratio of the rubber powder, ZDS and SMA is 10:0.6:1.0; the stirring and mixing time is 10 minutes; the melt blending condition is carried out at a temperature of 180°C; and the cooling is air cooling to room temperature;

[0030] 4) SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant and auxiliary agent are stirred and mixed, and a compatibilizer is added and stirred evenly, followed by melt blending, cooling, granulation and drying to obtain material B; wherein the auxiliary agent is calcium carbonate, polyethylene wax and polyethylene oxide mixed in a mass ratio of 3.0:1:1.2; the antioxidant is antioxidant 1010; the compatibilizer is N, N-diethylformamide; the mass ratio of SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant, auxiliary agent and compatibilizer is 30:30:30:90:10:20:5:3:15:10; the stirring and mixing time is 10 min; the melt blending condition is carried out at a temperature of 190° C.; the cooling is air cooling to room temperature;

[0031] 5) After blending material A and material B, extruding, cooling, granulating and drying, a TPE material is obtained; wherein the mass ratio of material A to material B is 4:30; the blending extrusion condition is melt extrusion at a temperature of 180° C. through a twin-screw extruder; and the cooling is cooling to room temperature using circulating water cooling.

[0032] Example 2

[0033] A method for preparing a composite TPE material comprises the following steps:

[0034] 1) crushing ABS and subjecting it to constant temperature treatment to obtain ABS prefabricated material; wherein the condition of the constant temperature treatment is at a temperature of 122° C. and a constant temperature of 52 hours;

[0035] 2) placing the hollow glass microspheres and the ABS prefabricated material in a sodium hydroxide solution, heating and stirring, and then filtering to obtain a pretreated material; wherein the heating and stirring conditions are at a temperature of 76° C., a speed of 460 r / min, and stirring for 1.1 h; the concentration of the sodium hydroxide solution is 0.36 mol / L; the mass ratio of the hollow glass microspheres, the ABS prefabricated material and the sodium hydroxide solution is 2.1:10.4:21; the density of the hollow glass microspheres is 0.50 g / cm 3 , particle size 60 μm;

[0036] 3) The rubber powder, ZDS and SMA are stirred and mixed, melt blended, cooled, granulated and dried to obtain material A; wherein the mass ratio of the rubber powder, ZDS and SMA is 10.4:0.64:1.1; the stirring and mixing time is 12 minutes; the melt blending condition is carried out at a temperature of 182°C; and the cooling is air cooling to room temperature;

[0037] 4) SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant and auxiliary agent are stirred and mixed, and a compatibilizer is added and stirred evenly, followed by melt blending, cooling, granulation and drying to obtain material B; wherein the auxiliary agent is calcium carbonate, polyethylene wax and polyethylene oxide mixed in a mass ratio of 3.1:1:1.26; the antioxidant is antioxidant 1010; the compatibilizer is N, N-diethylformamide; the mass ratio of SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant, auxiliary agent and compatibilizer is 30:31:31:92:11.5:21:6:3.2:16:11; the stirring and mixing time is 12 minutes; the melt blending condition is carried out at a temperature of 192°C; the cooling is air cooling to room temperature;

[0038] 5) After blending material A and material B, extruding, cooling, granulating and drying, a TPE material is obtained; wherein the mass ratio of material A to material B is 4.2:30.4; the blending extrusion condition is melt extrusion at a temperature of 182° C. through a twin-screw extruder; and the cooling is cooling to room temperature using circulating water cooling.

[0039] Example 3

[0040] A method for preparing a composite TPE material comprises the following steps:

[0041] 1) crushing ABS and subjecting it to constant temperature treatment to obtain ABS prefabricated material; wherein the condition of the constant temperature treatment is at a temperature of 124° C. and a constant temperature of 54 hours;

[0042] 2) The hollow glass microspheres and ABS prefabricated material are placed in a sodium hydroxide solution, heated and stirred, and then filtered to obtain a pretreated material; wherein the heating and stirring conditions are at a temperature of 77°C, a speed of 520r / min, and stirring for 1.2h; the concentration of the sodium hydroxide solution is 0.42moL / L; the mass ratio of the hollow glass microspheres, the ABS prefabricated material and the sodium hydroxide solution is 2.2:10.8:22; the density of the hollow glass microspheres is 0.50g / cm 3 , particle size 60 μm;

[0043] 3) The rubber powder, ZDS and SMA are stirred and mixed, melt blended, cooled, granulated and dried to obtain material A; wherein the mass ratio of the rubber powder, ZDS and SMA is 10.8:0.68:1.2; the stirring and mixing time is 14 minutes; the melt blending condition is carried out at a temperature of 184°C; and the cooling is air cooling to room temperature;

[0044] 4) SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant and auxiliary agent are stirred and mixed, and a compatibilizer is added and stirred evenly, followed by melt blending, cooling, granulation and drying to obtain material B; wherein the auxiliary agent is calcium carbonate, polyethylene wax and polyethylene oxide mixed in a mass ratio of 3.2:1:1.32; the antioxidant is antioxidant 1010; the compatibilizer is N, N-diethylformamide; the mass ratio of SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant, auxiliary agent and compatibilizer is 30:32:32:94:12:22:7:3.5:17:12; the stirring and mixing time is 14 minutes; the melt blending condition is carried out at a temperature of 194°C; the cooling is air cooling to room temperature;

[0045] 5) After blending material A and material B, extruding, cooling, granulating and drying, a TPE material is obtained; wherein the mass ratio of material A to material B is 4.4:30.8; the blending extrusion condition is melt extrusion at a temperature of 184° C. through a twin-screw extruder; and the cooling is cooling to room temperature using circulating water cooling.

[0046] Example 4

[0047] A method for preparing a composite TPE material comprises the following steps:

[0048] 1) crushing ABS and subjecting it to constant temperature treatment to obtain ABS prefabricated material; wherein the condition of the constant temperature treatment is at a temperature of 126° C. and a constant temperature of 56 hours;

[0049] 2) placing the hollow glass microspheres and the ABS prefabricated material in a sodium hydroxide solution, heating and stirring, and then filtering to obtain a pretreated material; wherein the heating and stirring conditions are at a temperature of 78°C, a speed of 580r / min, and stirring for 1.3h; the concentration of the sodium hydroxide solution is 0.48moL / L; the mass ratio of the hollow glass microspheres, the ABS prefabricated material and the sodium hydroxide solution is 2.3:11.2:23; the density of the hollow glass microspheres is 0.50g / cm 3 , particle size 60 μm;

[0050] 3) The rubber powder, ZDS and SMA are stirred and mixed, melt blended, cooled, granulated and dried to obtain material A; wherein the mass ratio of the rubber powder, ZDS and SMA is 11.2:0.72:1.3; the stirring and mixing time is 16 minutes; the melt blending condition is carried out at a temperature of 186°C; and the cooling is air cooling to room temperature;

[0051] 4) SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant and auxiliary agent are stirred and mixed, and a compatibilizer is added and stirred evenly, followed by melt blending, cooling, granulation and drying to obtain material B; wherein the auxiliary agent is calcium carbonate, polyethylene wax and polyethylene oxide mixed in a mass ratio of 3.3:1:1.38; the antioxidant is antioxidant 1010; the compatibilizer is N, N-diethylformamide; the mass ratio of SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant, auxiliary agent and compatibilizer is 30:33:33:96:14:23:8:4:18:13; the stirring and mixing time is 16 minutes; the melt blending condition is carried out at a temperature of 196°C; the cooling is air cooling to room temperature;

[0052] 5) After blending material A and material B, extruding, cooling, granulating and drying, a TPE material is obtained; wherein the mass ratio of material A to material B is 4.6:31.2; the blending extrusion condition is melt extrusion at a temperature of 186° C. through a twin-screw extruder; and the cooling is cooling to room temperature using circulating water cooling.

[0053] Example 5

[0054] A method for preparing a composite TPE material comprises the following steps:

[0055] 1) crushing ABS and subjecting it to constant temperature treatment to obtain ABS prefabricated material; wherein the condition of the constant temperature treatment is at a temperature of 128° C. and a constant temperature of 58 hours;

[0056] 2) placing the hollow glass microspheres and the ABS prefabricated material in a sodium hydroxide solution, heating and stirring, and then filtering to obtain a pretreated material; wherein the heating and stirring conditions are at a temperature of 79° C., a speed of 640 r / min, and stirring for 1.4 h; the concentration of the sodium hydroxide solution is 0.54 mol / L; the mass ratio of the hollow glass microspheres, the ABS prefabricated material and the sodium hydroxide solution is 2.4:11.6:24; the density of the hollow glass microspheres is 0.50 g / cm 3 , particle size 60 μm;

[0057] 3) The rubber powder, ZDS and SMA are stirred and mixed, melt blended, cooled, granulated and dried to obtain material A; wherein the mass ratio of the rubber powder, ZDS and SMA is 11.6:0.76:1.4; the stirring and mixing time is 18 minutes; the melt blending condition is carried out at a temperature of 188°C; and the cooling is air cooling to room temperature;

[0058] 4) After SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant and auxiliary agent are stirred and mixed, a compatibilizer is added and stirred evenly, and then melt blending, cooling, granulation and drying are performed to obtain material B; wherein the auxiliary agent is calcium carbonate, polyethylene wax and polyethylene oxide mixed in a mass ratio of 3.4:1:1.44; the antioxidant is antioxidant 1010; the compatibilizer is N, N-diethylformamide; the mass ratio of SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant, auxiliary agent and compatibilizer is 30:34:34:98:15:24:9:4.5:19:14; the stirring and mixing time is 18 minutes; the melt blending condition is carried out at a temperature of 198°C; the cooling is air cooling to room temperature;

[0059] 5) After blending material A and material B, extruding, cooling, granulating and drying, a TPE material is obtained; wherein the mass ratio of material A to material B is 4.8:31.6; the blending extrusion condition is melt extrusion at a temperature of 188° C. through a twin-screw extruder; and the cooling is cooling to room temperature using circulating water cooling.

[0060] Example 6

[0061] A method for preparing a composite TPE material comprises the following steps:

[0062] 1) crushing ABS and subjecting it to constant temperature treatment to obtain ABS prefabricated material; wherein the condition of the constant temperature treatment is at a temperature of 130° C. for 60 hours;

[0063] 2) placing the hollow glass microspheres and the ABS prefabricated material in a sodium hydroxide solution, heating and stirring, and then filtering to obtain a pretreated material; wherein the heating and stirring conditions are at a temperature of 80° C., a speed of 700 r / min, and stirring for 1.5 h; the concentration of the sodium hydroxide solution is 0.6 mol / L; the mass ratio of the hollow glass microspheres, the ABS prefabricated material and the sodium hydroxide solution is 2.5:12:25; the density of the hollow glass microspheres is 0.50 g / cm 3 , particle size 60 μm;

[0064] 3) The rubber powder, ZDS and SMA are stirred and mixed, melt blended, cooled, granulated and dried to obtain material A; wherein the mass ratio of the rubber powder, ZDS and SMA is 12:0.8:1.5; the stirring and mixing time is 20 minutes; the melt blending condition is carried out at a temperature of 190° C.; the cooling is air cooling to room temperature;

[0065] 4) SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant and auxiliary agent are stirred and mixed, and a compatibilizer is added and stirred evenly, followed by melt blending, cooling, granulation and drying to obtain material B; wherein the auxiliary agent is calcium carbonate, polyethylene wax and polyethylene oxide mixed in a mass ratio of 3.5:1:1.5; the antioxidant is antioxidant 1010; the compatibilizer is N, N-diethylformamide; the mass ratio of SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant, auxiliary agent and compatibilizer is 30:35:35:100:16:25:10:5:20:15; the stirring and mixing time is 20 minutes; the melt blending condition is carried out at a temperature of 200°C; the cooling is air cooling to room temperature;

[0066] 5) After blending material A and material B, extruding, cooling, granulating and drying, a TPE material is obtained; wherein the mass ratio of material A to material B is 5:32; the blending extrusion condition is melt extrusion at a temperature of 190° C. through a twin-screw extruder; and the cooling is cooling to room temperature using circulating water cooling.

[0067] Comparative Example 1

[0068] Compared with Example 4, the difference is that comparative example 1 does not use sodium hydroxide solution, and the other components, preparation steps and parameters are the same.

[0069] Comparative Example 2

[0070] Compared with Example 4, the difference is that ZDS is not used in Comparative Example 2, and the other components, preparation steps and parameters are the same.

[0071] Comparative Example 3

[0072] Compared with Example 4, the difference is that Comparative Example 3 does not use SMA, and the other components, preparation steps and parameters are the same.

[0073] Comparative Example 4

[0074] Compared with Example 4, the difference is that comparative example 4 does not use hollow glass microspheres, and the other components, preparation steps and parameters are the same.

[0075] Comparative Example 5

[0076] Compared with Example 4, the difference is that Comparative Example 5 uses TPEE instead of EVA, and the other components, preparation steps and parameters are the same.

[0077] Comparative Example 6

[0078] Compared with Example 4, the difference is that step 3) of Comparative Example 6 is:

[0079] 3) Mixing the rubber powder, ZDS and SMA to obtain material A;

[0080] The remaining components, preparation steps and parameters were the same.

[0081] Comparative Example 7

[0082] Compared with Example 4, the difference is that step 1) of Example 7 is not subjected to constant temperature treatment, and the other components, preparation steps and parameters are the same.

[0083] Comparative Example 8

[0084] Compared with Example 4, the difference is that the melt blending in step 3) of Comparative Example 8 is carried out at a temperature of 200° C.; the other components, preparation steps and parameters are the same.

[0085] The mechanical properties of Examples 1-6 and Comparative Examples 1-8 were tested (GB / T528-1998), and the test results are shown in Table 1.

[0086] Table 1

[0087] Tensile strength(MPa) Elongation at break (%) Example 1 19.7 716 Example 2 19.6 713 Example 3 19.9 719 Example 4 20.2 723 Example 5 19.6 715 Example 6 19.8 718 Comparative Example 1 14.5 621 Comparative Example 2 16.1 643 Comparative Example 3 13.2 606 Comparative Example 4 14.8 629 Comparative Example 5 13.5 611 Comparative Example 6 11.8 575 Comparative Example 7 16.5 650 Comparative Example 8 18.1 663

[0088] It can be seen from the test results in Table 1 that, compared with Comparative Examples 1-8, the mechanical properties of the TPE materials prepared in Examples 1-6 are significantly better than those in Comparative Examples 1-8.

[0089] By comparing Examples 1-6 with Comparative Examples 1, 4, and 7 and combining with the analysis in Table 1, it can be seen that the constant temperature treatment can promote the PB phase in ABS to generate more hydroxyl groups, and the surfaces of ABS and hollow glass microspheres are slightly etched and hydroxylated by sodium hydroxide solution to increase their surface roughness and the number of hydroxyl groups. The improvement of the surface roughness is conducive to enhancing the compatibility between the polymer materials, and the increase in the number of hydroxyl groups is conducive to increasing the crosslinking density of the TPE material, thereby significantly improving the mechanical properties.

[0090] By comparing Examples 1-6 with Comparative Examples 2, 3, 5 and 6 and combining with the analysis in Table 1, it can be seen that the compatibility between ZDS and the rubber powder is increased by using the non-polar benzene ring group and the polar carboxylic acid group in the structure of SMA, and the introduction of SMA and ZDS increases the compatibility between the rubber powder and ABS. Specifically, the anhydride group in SMA can react with the hydroxyl group of ABS and the hollow glass microspheres, and the free radicals generated by ZDS can be grafted with the PB phase of ABS, which significantly improves the interaction force between material A and material B during the hot melt process. In addition, the EVA resin structure has both polar groups and non-polar groups. The polar part can be compatible with the hydroxyl groups of ABS and the hollow glass microspheres, and the non-polar part can be compatible with the rubber powder, which effectively improves the compatibility between the components in the TPE composite material, enhances the bonding force between the materials, and thus significantly improves the compatibility of the TPE system.

[0091] By comparing Examples 1-6 with Comparative Example 8 and analyzing in combination with Table 1, it can be seen that too high a hot melt blending temperature has a great influence on the performance of the rubber powder modified TPE material. When the temperature is too high, the elastic modulus of the rubber powder will be reduced, thereby affecting the mechanical properties of the TPE material.

[0092] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a composite TPE material, characterized in that: The preparation method comprises the following steps: 1) crushing ABS and subjecting it to constant temperature treatment to obtain ABS prefabricated material; 2) placing the hollow glass microspheres and the ABS prefabricated material in a sodium hydroxide solution, heating and stirring, and then filtering to obtain a pretreated material; the mass ratio of the hollow glass microspheres, the ABS prefabricated material and the sodium hydroxide solution is 2.0-2.5:10-12:20-25; 3) mixing the rubber powder, ZDS and SMA, melt blending, cooling, granulating and drying to obtain material A; the ZDS is zinc sorbate; the mass ratio of the rubber powder, ZDS and SMA is 10-12:0.6-0.8:1.0-1.5; 4) SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant and auxiliary agent are stirred and mixed, and a compatibilizer is added and stirred evenly, and then melt blending, cooling, granulation and drying are performed to obtain material B; the mass ratio of SEBS, white oil, PPO, TPEE, EVA, pretreatment material, stearic acid, antioxidant, auxiliary agent and compatibilizer is 30:30-35:30-35:90-100:10-16:20-25:5-10:3-5:15-20:10-15; the auxiliary agent is a mixture of calcium carbonate, polyethylene wax and polyethylene oxide in a mass ratio of 3.0-3.5:1:1.2-1.5; 5) The material A and the material B are blended, extruded, cooled, granulated and dried to obtain a TPE material; the mass ratio of the material A to the material B is 4-5:30-32.

2. The method for preparing a composite TPE material according to claim 1, characterized in that: In step 1), the isothermal treatment is carried out at 120-130° C. for 50-60 hours.

3. The method for preparing a composite TPE material according to claim 1, characterized in that: In step 2), the heating and stirring conditions are 75-80°C, 400-700r / min, and stirring for 1.0-1.5h; the concentration of the sodium hydroxide solution is 0.3-0.6moL / L; and the hollow glass microspheres are selected from at least one of a density of 0.12-0.70g / cm3 and a particle size of 5-100μm.

4. The method for preparing a composite TPE material according to claim 1, characterized in that: In step 3), the stirring and mixing time is 10-20 minutes; the melt blending is carried out at a temperature of 180-190° C.; and the cooling is air cooling to room temperature.

5. The method for preparing a composite TPE material according to claim 1, characterized in that: In step 4), the antioxidant is one or both of antioxidant 1010 and antioxidant PS802; and the compatibilizer is N,N-diethylformamide.

6. The method for preparing a composite TPE material according to claim 1, characterized in that: In step 4), the stirring and mixing time is 10-20 minutes; the melt blending condition is carried out at a temperature of 190-200° C.; and the cooling is air cooling to room temperature.

7. The method for preparing a composite TPE material according to claim 1, characterized in that: In step 5), the blending extrusion is performed under the conditions of melt extrusion at a temperature of 180-190° C. through a twin-screw extruder; and the cooling is performed by cooling to room temperature using circulating water cooling.

8. A composite TPE material obtained by the preparation method according to any one of claims 1 to 7.