High flowability thermal conductive silicone paste and preparation method thereof

By using a multi-component combination method, a cross-linked network is formed using polymers with specific structures and treated alumina fillers, which resolves the contradiction between the flowability and thermal conductivity of thermal conductive grease, achieving good flowability and high thermal conductivity of thermal conductive grease under high filling load.

CN118085581BActive Publication Date: 2026-11-24ZHEJIANG YINGKE NEW MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410304881.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-18
Publication Date
2026-11-24
Estimated Expiration
2044-03-18

AI Technical Summary

Technical Problem

Existing technologies struggle to maintain the flowability and coating performance of thermally conductive silicone paste while ensuring a high thermal conductivity filler load, leading to problems such as cracking, powdering, or difficulty in application.

Method used

A multi-component approach is adopted, using dimethyl vinyl-terminated polydimethylsiloxane, treated alumina filler, and cross-branched polysiloxane. Through compatibility and cross-linking network formation, the dispersibility and flowability of the filler in silicone paste are improved.

Benefits of technology

This invention achieves good flowability and high thermal conductivity in thermally conductive silicone grease under high filling load, resolves the contradiction between flowability and thermal conductivity, and improves the thermal conductivity of thermal interface materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118085581B_ABST
    Figure CN118085581B_ABST
Patent Text Reader

Abstract

This invention relates to the field of thermal interface materials technology, and discloses a high-flow thermally conductive silicone grease and its preparation method. The thermally conductive silicone grease includes raw materials: component C1, component C2, component C3, and component C4; component C1 is a dimethyl vinyl-terminated polydimethylsiloxane, component C2 is a polymer with the structure shown in (II), and component C3 is a polymer with the structure shown in (III). In this invention, component C2 is used as a surface modifier for component C4, component C1 is used as the polymer matrix, and component C3 is used as a flowability modifier. The resulting thermally conductive silicone grease has lower viscosity and better flowability, and can uniformly disperse more thermally conductive fillers into the organosilicon matrix to obtain a silicone grease with high filler volume fraction and high thermal conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thermal interface materials technology, specifically to a highly fluid thermally conductive silicone grease and its preparation method. Background Technology

[0002] Thermally conductive grease is a flexible composite material coated between the interface of a heat source and a heat dissipation device. Applying thermally conductive grease between the heat source and the heat dissipation device effectively mitigates the adverse effects of low thermal conductivity air on heat conduction, thus ensuring the normal operation and extending the service life of heat-generating devices (such as communication chips, communication base stations, power batteries, and high-power LED lighting devices). This, in turn, ensures the normal use of various devices or facilities that install these heat-generating devices, such as mobile phones, computers, and electric vehicles.

[0003] Thermally conductive silicone grease is a composite material composed of linear polydimethylsiloxane as the polymer matrix and various fillers with high thermal conductivity. The polydimethylsiloxane acts as an adhesive, "bonding" the various fillers together and allowing it to be applied flexibly and easily to areas requiring heat conduction. With the addition of thermally conductive fillers to the silicone grease composite, the thermal conductivity of the grease gradually increases, and its heat transfer efficiency also increases.

[0004] Fillers with high thermal conductivity are typically metals, metal oxides, metal compounds, or phase change alloys. The surface and interfacial properties of these materials are completely different from those of linear polydimethylsiloxanes used as polymer matrices, making it difficult to uniformly disperse these high-thermal-conductivity fillers within linear polydimethylsiloxanes with high packing loads. Although spherical or near-spherical Al2O3 has a relatively low thermal conductivity compared to other high-thermal-conductivity fillers, its low price makes it widely used as a thermally conductive filler in various thermally conductive materials. Unlike other types of thermally conductive fillers, spherical or near-spherical Al2O3 also contains hydroxyl groups on its surface. Since hydroxyl groups are hydrophilic, while linear polydimethylsiloxanes are hydrophobic, dispersing spherical or near-spherical Al2O3 within hydrophobic linear polydimethylsiloxanes is very difficult, making it challenging to obtain alumina-based thermally conductive greases with high packing loads and high thermal conductivity.

[0005] To improve the surface properties of spherical or near-spherical Al2O3, industry and academia typically use coupling agents or other surface treatment agents to treat the fillers. This aims to improve the compatibility between the fillers and the organosilicon polymer matrix, increase the amount of thermally conductive fillers in the polymer matrix, and improve the thermal conductivity of the thermal interface material. However, as the amount of inorganic fillers increases, the viscosity of the thermally conductive silicone grease prepared using the above techniques also increases rapidly, making it difficult to obtain a thermally conductive silicone grease that meets both the coating performance required for application and has a high thermal conductivity.

[0006] Branched polymers possess unique topological structures that significantly influence their structure, kinetics, and rheological properties. Compared to linear polymers, branched polymers exhibit numerous intramolecular cavities and terminal groups, along with superior chain flexibility, lower entanglement, and a non-monotonic increase in viscosity with molecular weight. The main topological structures of polymers include star-shaped, comb-shaped, bottle-brush-shaped, and ring-shaped structures. The earliest and most thoroughly studied topological structure is the star-shaped polymer with a single branch point, which is also the simplest branched polymer.

[0007] Star polymers are branched polymers containing more than three chains (arms) where the main chain and branches cannot be distinguished. Each chain segment or arm is chemically bonded to a single carbon atom, and the core size is much smaller than the overall polymer size. Star polymers can be synthesized using either a core-to-arm or arm-to-core approach, or even through grafting. Each method has its advantages and disadvantages, and the appropriate synthesis method must be selected based on the properties and target application when designing star polymers. Ring-opening polymerization, living anionic or cationic polymerization, living radical polymerization, and ring-opening metathesis polymerization are commonly used methods for polymer synthesis today.

[0008] The literature (Acta Petrolei Sinica (Petroleum Processing), 2000, 16(01): 40-46) reported star polymers with different molecular structures and their application in the deplasm reduction and viscosity reduction treatment of different oil products and crude oils. It was found that star polymers can significantly reduce the viscosity of heavy oil; as the number of branches increases and the spatial structure becomes more regular, the viscosity reduction performance is better. In addition to the star structure, other polymer structures also have certain effects on the viscosity reduction of heavy oil.

[0009] Another paper (Applied Chemical Engineering, 2012, 41(03): 469-472) discloses a dendritic viscosity reducer. When added at 1 wt%, it achieves the best viscosity reduction effect on heavy oil, with a viscosity reduction rate of 69.2%. In addition, other papers (Li Cuiqin. Molecular Design and Performance Study of Dendritic Acrylates [D]. Daqing: Daqing Petroleum Institute, 2004) also disclose a polyamide-amine dendritic macromolecule. This macromolecule uses ethylenediamine as the core, and the three half-generation PAMAMs obtained all show a certain viscosity reduction effect on heavy oil. For example, when 0.6% of the mass of heavy oil PAMAM is added at 70℃, after 60 min, the 2.5 generation PAMAM is found to have the best viscosity reduction effect on heavy oil, with a viscosity reduction value of 28.2%.

[0010] Synthesized dendritic long-chain acrylic ester polymers (Li Cuiqin. Molecular Design and Performance Study of Dendritic Acrylates [D]. Daqing: Daqing Petroleum Institute, 2004.) can also be used as viscosity reducers for oil products. When the addition amount is 0.6%, the viscosity reduction effect of heavy oil is optimal. The viscosity reduction rate of 0.5 generation dendritic octyl ester is 26.2%, dodecyl ester is 28.3%, and octadecyl ester is 32.4%. In addition, comb-type polymers with different side chain modifications and spatial topological structures (Qian Huiqin. Study on the Influence of Side Chain Structure of Comb-type Copolymers on Oil Flowability [D]. Shanghai: East China University of Science and Technology, 2012.) can also reduce the viscosity of crude oil, so that crude oil at low temperature still has good flowability.

[0011] Although the literature discloses methods for synthesizing branched polymers with spatial topological structures and their applications in reducing crude oil viscosity, the molecular structure of linear polydimethylsiloxane differs from that of carbon-based polymers. Therefore, mixing these topologically structured polymers with linear polydimethylsiloxanes not only fails to reduce the viscosity of the linear polydimethylsiloxanes but also results in a completely layered polymer solution due to the significant difference in their solubility parameters. This makes achieving high fluidity in silicone grease structures difficult.

[0012] CN113896894A discloses a method for preparing cross-shaped dimethyl vinyl-terminated polysiloxane. This branched crosslinking agent has the characteristics of preventing the vinyl chain segments from becoming too concentrated and having high reactivity. When used in high-temperature vulcanized silicone rubber, it can produce high-temperature vulcanized silicone rubber with tensile strength between 8.2 and 10.5 MPa, tear strength above 24.7 kN / m, and elongation at break above 830%, without the need for two-stage vulcanization.

[0013] Although relevant literature discloses the synthesis method of cross-shaped dimethyl vinyl-terminated polysiloxanes and their effect on improving the mechanical properties of high-temperature vulcanized silicone rubber, the influence of this special structure on the viscosity of the high-temperature vulcanized silicone rubber system and the extent of such influence are not disclosed. Therefore, how to solve the contradiction between the fluidity and thermal conductivity of silicone paste under high filling load of thermally conductive fillers remains an urgent problem to be solved in the thermal interface materials industry. Summary of the Invention

[0014] This invention addresses the technical problem of thermal grease losing fluidity due to high Al2O3 content, resulting in cracking, powdering, or difficulty in application. It provides a high-fluidity thermal grease that, through the combination of multiple components, maintains high Al2O3 content, high thermal conductivity, and good fluidity.

[0015] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0016] A high-flow thermal conductive grease, the thermal conductive grease comprising raw materials: component C1, component C2, component C3 and component C4;

[0017] Component C1 is a dimethyl vinyl-terminated polydimethylsiloxane with the structure shown in formula (I); where a is any natural number from 3 to 300;

[0018]

[0019] Component C2 is a polymer with the structure shown in (II), wherein Ra is methyl, butyl, phenyl, or trimethylsilylmethyl (Me3SiCH2-); Rb is methyl, ethyl, methoxy, or ethoxy; Rc is methyl, ethyl, methoxy, or ethoxy; Rd is methyl, ethyl, methoxy, or ethoxy; and at least one of the terminal groups Rb, Rc, and Rd contains a methoxy or ethoxy group; X is absent or is a (CH2)z group, where z is a positive integer from 2 to 6; and n is any natural number from 1 to 500.

[0020]

[0021] Component C3 is a polymer with the structure shown in (III), where m is any natural number from 1 to 500;

[0022]

[0023] Component C4 is aluminum oxide.

[0024] In this invention, component C1 serves as the polymer matrix material, providing coating and film formation for component C4 after treatment with component C2. This results in tightly packed C4 that is less prone to pulverization, while also eliminating the decrease in thermal conductivity of the thermally conductive silicone paste caused by micro-bubble inclusions. Component C3 has the same polymer backbone structure (Me2SiO chain segments) and the same end group structure (Me2ViSiO) as component C1. 1 / 2 Both components have good compatibility and similar solubility parameters. Both can undergo hydrosilylation reactions with small molecules or polymers containing Si-H bonds to form a uniform cross-linked network. Another prominent feature of component C3 is its cross-shaped spatial structure. Not only can its helical molecular chains interpenetrate with the helical molecular chains of component C1, but this cross-shaped branched structure also facilitates the accommodation of component C4 filler particles treated with component C2. This results in good sliding properties of the C4 filler particles treated with component C2 between component C3 molecular chains and between the helical molecular chains of component C3 and component C1.

[0025] Through the synergistic effect of the above components, namely by treating C4 filler with component C2 to increase the filling load of C4 filler, and by the unique molecular configuration of component C3 and the extension effect of the polymer chains of components C1 and C3, the complex viscosity of C4 with high filling load in the composite material system is reduced, which effectively improves the fluidity of thermal conductive silicone grease.

[0026] Preferably, the viscosity of component C1 at 25°C is 10–1000 mPa·s.

[0027] Preferably, in component C3, m is 1–300, the molecular weight is 720–90000 g / mol, and the viscosity at 25°C is 3–2000 mPa·s; more preferably, m is 5–50, the molecular weight is 1900–16000 g / mol, and the viscosity at 25°C is 10–200 mPa·s. This molecular weight and viscosity of C3 are suitable, effectively accommodating C4 filler particles treated with C2 while ensuring the fluidity of the silicone paste.

[0028] Preferably, n in component C2 is 1–50, and the molecular weight is 250–4000 g / mol; more preferably, n in C2 is 3–45, and the molecular weight is 400–3550 g / mol. When the degree of polymerization of component C2 is small or the molecular weight is small, the polysiloxane segments grafted onto the surface of component C4 treated with component C2 are short. In this case, component C4 has poor dispersibility in components C3 and C1, is unstable, and is prone to sedimentation. When the degree of polymerization of component C2 is large or the molecular weight is large, the concentration of alkoxy functional groups in component C2 is low, the reactivity is low, and it cannot effectively reduce the surface content of component C4, resulting in poor compatibility between component C4 and components C1 and C3.

[0029] Preferably, in component C2, Ra is methyl, X is -(CH2)2-, and Rb, Rc, and Rd are all methoxy groups;

[0030] Preferably, the mass ratio of component C1 to component C3 is 3 to 20:1. More preferably, the mass ratio of component C1 to component C3 is 3 to 10:1.

[0031] Preferably, the sum of the masses of components C1 and C3 is 100 parts by weight, the amount of component C4 is 400 to 2800 parts by weight, and the amount of component C2 is 1.25 to 145 parts by weight.

[0032] The component C4 is a mixture of spherical or near-spherical alumina with average particle sizes A1, A2 and A3;

[0033] A1 is 0.1–1.0 μm, A2 is 2.0–10.0 μm, and A3 is 50–500 μm;

[0034] The mass ratio of oxides with particle sizes of A1, A2 and A3 in component C4 is 1-4:2-8:5-15.

[0035] The thermally conductive silicone grease of the present invention has a viscosity of 1.5 × 10⁻⁶ at 0.1 Hz. 5 ~4.0×10 5 Pa·s, at 1.0 Hz, is 1.0 × 10⁻⁶. 4 ~8.0×10 4 Pa·s at 10.0 Hz is 1.0 × 10⁻⁶. 3 ~5.0×10 3 Pa·s at 100.0 Hz is 1.0 × 10⁻⁶. 2 ~5.0×10 2 Pa·s; thermal conductivity is between 5.90 and 8.10 W / (m·K), exhibiting high fluidity and thermal conductivity.

[0036] The present invention also provides a method for preparing the high-flowability thermal conductive grease, comprising mechanically mixing components C1, C2, C3 and C4 and removing air bubbles under vacuum to obtain the thermal conductive grease.

[0037] Preferably, component C1 and component C3 are mixed at room temperature, then component C2 is added and dispersed, and finally component C4 is added in batches or all at once for high-speed dispersion and mixing. After degassing, the thermally conductive silicone paste is prepared.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) Through the synergistic effect of each component, the prepared thermally conductive silicone grease has both high thermal conductivity and good fluidity;

[0040] (2) By adopting the technical solution of the present invention, the filling coefficient of thermally conductive filler can be further increased while the thermally conductive silicone grease has good fluidity, thereby obtaining a preparation method for forming a high thermal conductivity thermally conductive silicone grease and improving the thermal conductivity of the thermal interface material.

[0041] (3) Compared with the prior art, the method disclosed in this invention can uniformly disperse more thermally conductive fillers into the organosilicon matrix to obtain silicone paste with high filler volume fraction and high thermal conductivity. Attached Figure Description

[0042] Figure 1 The relationship between the complex viscosity η* of the thermal grease in Examples 1-7 and Comparative Example 1 and frequency.

[0043] Figure 2 The relationship between the complex viscosity η* of the thermally conductive silicone grease prepared in Examples 1, 8-12 and frequency. Detailed Implementation

[0044] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Modifications or equivalent substitutions made by those skilled in the art based on their understanding of the technical solutions of this invention, without departing from the spirit and scope of the invention, should be covered within the protection scope of this invention.

[0045] Unless otherwise specified, all raw materials used in this invention are commercially available or commonly used in the field. Unless otherwise specified, the methods in the following embodiments are conventional methods in the field.

[0046] Complex viscosity η*: Dynamic rheological behavior was tested using an advanced rotational rheometer (ARES-G2, TA Instruments, USA) in flat plate mode. The dynamic frequency scan was performed from high frequency to low frequency, with the set frequency range, strain, and temperature being 0.1–100 Hz, 0.05%, and 30 °C, respectively.

[0047] Thermal conductivity: The thermal conductivity of the thermal grease was tested using a DRL-III thermal conductivity tester manufactured by Xiangtan Xiangyi Instrument Co., Ltd., according to the ASTM D5470 method. The heating plate was set to 50℃ and the sample thickness was 1-2 mm.

[0048] Component C1 is a commercially available dimethylvinyl-terminated polydimethylsiloxane. Component C2 is a commercially available α-trimethylsiloxy-ω-trimethoxysilylethyl-terminated polydimethylsiloxane. Component C3 is a cross-shaped dimethylvinyl-terminated polydimethylsiloxane prepared according to CN113896894A. Component C4 is a commercially available spherical Al2O3 particle.

[0049] Example 1 Thermal grease sample 1

[0050] At room temperature, 83.3 parts by weight of a dimethyl vinyl-terminated polydimethylsiloxane (component C1, structural formula (I)) with a viscosity of 50 mPa·s and 16.7 parts by weight of a dimethyl vinyl siloxy-terminated cross-branched polysiloxane (component C3) with a structure as shown in formula (III), a degree of polymerization m=16, an NMR molecular weight of 5169 g / mol, a PDI value of 1.90, and a viscosity of 45.00 mPa·s at 25℃ were added to a vacuum degassing mixer (the mass ratio of component C1 to component C3 was 5:1). The mixture was stirred and degassed at 1800 rpm and -99.5 kPa for 5 min to ensure uniform mixing.

[0051] Add 31.6 parts by weight of α-trimethylsiloxy-ω-trimethoxysilylethyl-terminated polydimethylsiloxane (structural formula shown in formula (II), where Ra is methyl, X is -(CH2)2-, and Rb, Rc and Rd are all methoxy) with a molecular weight of 960 g / mol and a degree of polymerization of 9 to the mixture in the above steps, and then stir and degas at 1800 rpm and -99.5 kPa for 5 min;

[0052] Then, 395.8 parts by weight of spherical alumina with an average particle size of 0.4 μm, 659.7 parts by weight of spherical alumina with an average particle size of 3.0 μm and 1187.5 parts by weight of spherical alumina with an average particle size of 120 μm were added at one time. The mixture was stirred and degassed twice in a vacuum degassed mixer at 1800 rpm and -99.5 kPa, with each treatment lasting 2 to 3 minutes, to prepare the thermally conductive silicone grease.

[0053] The densities of components C1 and C3 are both 0.96 g / cm³. 3 The density of spherical alumina with different particle sizes was calculated to be 4.0 g / cm³. 3 The calculation showed that the volume fraction of aluminum oxide in the thermal grease was 84.3%.

[0054] Examples 2 to 7: Thermal grease sample 2 to thermal grease sample 8

[0055] By changing only the relative amounts of components C1 and C3, without changing the amounts of the other components, thermal greases with different ratios of components C1 and C3 were prepared according to the same procedure and steps as in Example 1. The amounts are shown in Table 1 below.

[0056] Table 1. Composition of thermally conductive silicone grease prepared in Examples 2 to 7 (parts by weight)

[0057]

[0058] Example 8: Preparation of thermally conductive silicone grease with a degree of polymerization m of component C3 of 10

[0059] The thermal grease of Example 8 was prepared by replacing component C3 in Example 1 with component C3, which has a degree of polymerization m=10, an NMR molecular weight of 3393 g / mol, a PDI value of 2.04, and a viscosity of 17.25 mPa·s at 25°C, without changing the amount of other components.

[0060] Example 9: Preparation of thermally conductive silicone grease with a degree of polymerization m of component C3 of 25.

[0061] The thermal grease of Example 9 was prepared by replacing component C3 in Example 1 with component C3, which has a degree of polymerization m=25, NMR molecular weight of 7833 g / mol, PDI value of 1.69, and viscosity of 49.75 mPa·s at 25°C, without changing the amount of other components, following the same processing steps as in Example 1.

[0062] Example 10: Preparation of thermally conductive silicone grease with a degree of polymerization m of component C3 of 33

[0063] The thermal grease of Example 10 was prepared by replacing component C3 in Example 1 with component C3, which has a degree of polymerization m=33, an NMR molecular weight of 10200 g / mol, a PDI value of 1.90, and a viscosity of 68.25 mPa·s at 25°C, without changing the amount of other components.

[0064] Example 11 Preparation of thermally conductive silicone grease with a degree of polymerization of C3 m = 50

[0065] The thermal grease of Example 11 was prepared by replacing component C3 in Example 1 with component C3, which has a degree of polymerization m=50, NMR molecular weight of 15233 g / mol, PDI value of 2.05, and viscosity of 165.30 mPa·s at 25°C, without changing the amount of other components.

[0066] Example 12 Preparation of thermally conductive silicone grease with a degree of polymerization m of component C3 of 239

[0067] The thermal grease of Example 12 was prepared by replacing component C3 in Example 1 with component C3, which has a degree of polymerization m=239, NMR molecular weight of 71177 g / mol, PDI value of 2.40, and viscosity of 1010 mPa·s at 25°C, without changing the amount of other components, and following the same processing steps as in Example 12.

[0068] Comparative Example 1: Thermal grease prepared without component C3

[0069] Using 100 parts by weight of dimethyl vinyl-terminated polydimethylsiloxane (component C1) with a viscosity of 50 mPa·s to replace components C1 and C3 in Example 1, without changing the amount of the other components, thermal grease without component C3 was prepared according to the same procedure and steps as in Example 1.

[0070] Performance testing

[0071] The complex viscosity η of the thermal greases prepared in Examples 1 to 7 and Comparative Example 1 was tested using an advanced rotational rheometer (ARES-G2). * The relationship between frequency and frequency is listed below. Figure 1 The complex viscosity η of the thermally conductive silicone greases prepared in Examples 1, 8 to 12 was measured. * The relationship between frequency and frequency is listed below. Figure 2 middle.

[0072] The thermal conductivity of the thermal greases prepared in Examples 1 to 7 and Comparative Example 1 was tested using a DRL-III thermal conductivity tester manufactured by Xiangtan Xiangyi Instrument Co., Ltd., according to ASTM D5470 method. The results are listed in Table 2. The thermal conductivity of the thermal greases prepared in Examples 8 to 12 was measured, and the results are listed in Table 3.

[0073] Table 2 shows the thermal conductivity of the thermal greases prepared in Examples 1 to 7 and Comparative Example 1.

[0074]

[0075]

[0076] Table 3. Thermal conductivity of the thermal greases prepared in Examples 8 to 12

[0077]

[0078] Depend on Figure 1It is evident that adding a dimethyl vinyl-terminated, cross-branched polysiloxane (component C3) to thermal grease significantly reduces its complex viscosity. Especially when the mass ratio of component C1 to component C3 is 10:1, the prepared thermal grease exhibits the lowest complex viscosity and best performance across different frequency ranges. Figure 2 It is evident that the degree of polymerization (m) of the dimethyl vinyl-terminated cross-branched polysiloxane (component C3) added to the thermal grease can significantly reduce the viscosity of the thermal grease in the range of 10 to 239. In particular, component C3 has an excellent viscosity-reducing effect in the range of 16 to 50.

[0079] Based on the test results of complex viscosity and thermal conductivity shown in Tables 2 and 3, it can be seen that when component C3 with a degree of polymerization m in the range of 16 to 50 is used in the thermal grease, the thermal conductivity of the prepared thermal grease does not change much compared with that without component C3, but the fluidity of the thermal grease is significantly improved.

[0080] The basic principles, main features, and advantages of this application have been described above. Those skilled in the art should understand that this application is not limited to the above embodiments. The embodiments and descriptions in the specification are merely the principles of this application. Various changes and modifications can be made to this application without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claims. The scope of protection claimed by this application is defined by the appended claims and their equivalents.

Claims

1. A high-flowability thermally conductive silicone grease, characterized in that, The thermally conductive silicone paste comprises the following raw materials: component C1, component C2, component C3, and component C4; Component C1 is a dimethyl vinyl-terminated polydimethylsiloxane with the structure shown in formula (I); where a is any natural number from 3 to 300; (I) Component C2 is a polymer with the structure shown in (II), wherein Ra is methyl, butyl, phenyl, or trimethylsilylmethyl (Me3SiCH2-); Rb is methyl, ethyl, methoxy, or ethoxy; Rc is methyl, ethyl, methoxy, or ethoxy; Rd is methyl, ethyl, methoxy, or ethoxy; and at least one of the terminal groups Rb, Rc, and Rd contains a methoxy or ethoxy group; X is absent or is a (CH2)z group, where z is a positive integer from 2 to 6; and n is any natural number from 1 to 500. (II) Component C3 is a polymer with the structure shown in (III), where m is any natural number from 10 to 239; (III) Component C4 is aluminum oxide.

2. The high-flowability thermally conductive silicone grease according to claim 1, characterized in that, The viscosity of component C1 at 25°C is 10~1000 mPa·s.

3. The high-flow thermally conductive silicone grease according to claim 1, characterized in that, In component C3, m is 10~50, molecular weight is 1900~16000 g / mol, and viscosity at 25℃ is 10~200 mPa.s.

4. The high-flow thermally conductive silicone grease according to claim 1, characterized in that, In component C2, n is 1~50 and the molecular weight is 250~4000 g / mol.

5. The high-flow thermally conductive silicone grease according to claim 1, characterized in that, In component C2, n is 3~45 and the molecular weight is 400~3550 g / mol.

6. The high-flow thermally conductive silicone grease according to claim 1, characterized in that, In component C2, Ra is methyl, X is -(CH2)2-, and Rb, Rc, and Rd are all methoxy.

7. The high-flow thermally conductive silicone grease according to claim 1, characterized in that, The mass ratio of component C1 to component C3 is 3~20:1; the sum of the masses of component C1 and component C3 is 100 parts by weight, the amount of component C4 is 400~2800 parts by weight, and the amount of component C2 is 1.25 parts by weight~145 parts by weight.

8. The high-flow thermally conductive silicone grease according to claim 1, characterized in that, The component C4 is a mixture of spherical or near-spherical alumina with average particle sizes A1, A2 and A3; A1 is 0.1~1.0 μm, A2 is 2.0~10.0 μm, and A3 is 50~500 μm; The mass ratio of alumina particles of A1, A2 and A3 in component C4 is 1~4:2~8:5~15.

9. The high-flow thermally conductive silicone grease according to claim 1, characterized in that, The viscosity of the thermally conductive silicone paste is 1.5 × 10⁻⁶ at 0.1 Hz. 5 ~4.0×10 5 Pa·s, at 1.0 Hz, is 1.0 × 10⁻⁶. 4 ~8.0×10 4 Pa·s at 10.0 Hz is 1.0 × 10⁻⁶. 3 ~5.0×10 3 Pa·s at 100.0 Hz is 1.0 × 10⁻⁶. 2 ~5.0×10 2 Pa.s; The thermal conductivity of the thermally conductive grease is between 5.90 and 8.10 W / (m·K).

10. The method for preparing the high-flowability thermally conductive silicone grease according to claim 1, characterized in that, The process includes the following steps: mechanically mixing components C1, C2, C3, and C4 and removing air bubbles under vacuum to obtain the thermally conductive silicone paste.

11. The method for preparing the high-flowability thermally conductive silicone grease according to claim 10, characterized in that, The process includes the following steps: mixing component C1 and component C3 at room temperature, then adding component C2 and dispersing the mixture, and finally adding component C4 in batches or all at once for high-speed dispersion and mixing, followed by degassing to remove air bubbles to prepare the thermally conductive silicone paste.

Citation Information

Patent Citations

  • Branched cross-linking agent as well as preparation method and application thereof

    CN113896894A