A method for recycling and repairing a waste lithium ion battery graphite negative plate
By combining ultrasonic treatment, plasma ball milling, and calcination, the problem of repairing graphite anode sheets from waste lithium-ion batteries has been solved, achieving an efficient and environmentally friendly regeneration process and improving the electrochemical performance of the regenerated graphite anode material.
Patent Information
- Application Number
- CN202410146492.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-02
AI Technical Summary
Existing technologies are insufficient for efficiently repairing graphite anode sheets from waste lithium-ion batteries, resulting in their inability to be directly reused after their cycle life ends. Furthermore, the recycling process involves secondary pollution and high energy consumption.
A combination of ultrasonic, plasma ball milling, and calcination methods was used to deposit graphene oxide and form a carbon coating on graphite anode sheets from waste lithium-ion batteries. Graphene oxide was generated on the graphite surface through plasma ball milling, and the graphite structure and properties were restored by calcination.
It enables rapid repair of waste graphite in a short period of time, reduces processing costs, improves the electrochemical performance of recycled graphite anode materials, and does not generate secondary pollution.
Smart Images

Figure CN118099582B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrode material repair and regeneration technology, and particularly relates to a method for regenerating and repairing graphite anode sheets from waste lithium-ion batteries. Background Technology
[0002] The mission to reduce greenhouse gas emissions and improve environmental sustainability is accelerating the electric vehicle market. Many countries are phasing out internal combustion engines and automobile sales in the coming decades, based on significantly tightened fuel emission standards. To achieve these goals, lithium-ion batteries (LIBs) are poised to become a key energy storage and conversion technology due to their advantages such as high energy density, high specific capacity, low cost, and low self-discharge rate. However, the cycle life of lithium-ion batteries is only 3-10 years. It is estimated that between 2015 and 2040, the amount of waste LIBs will reach 21 million tons. Unfortunately, less than 5% of waste LIBs are fully reused. Furthermore, current recycling processes mainly focus on valuable elements in waste cathode materials, such as Li, Co, and Ni, while waste graphite anode materials are largely neglected. Graphite is currently the primary choice for LIB anodes due to its low price, stable cycle performance, high specific capacitance, and low operating potential. Typically, it accounts for about 20% of the mass and 15% of the total cost of LIBs, which would make the waste graphite recycling market worth $100 billion. Therefore, developing efficient graphite regeneration technology is of great significance.
[0003] Waste graphite contains a certain amount of impurities, mainly including binders, SEI films, and residual electrolytes. Furthermore, the long-term charge-discharge cycle of LIBs damages the crystal structure of waste graphite, leading to a sharp decline in its capacity. Therefore, waste graphite cannot be directly reused without any treatment or regeneration. Several graphite recycling processes have been proposed, such as catalytic graphitization, hydrometallurgy, sulfuric acid leaching, and high-temperature treatment. However, hydrometallurgy cannot remove complex organic and inorganic impurities and is inefficient. Using strong acids is almost ineffective in repairing structural defects and generates wastewater. Other methods require high temperatures (2800-3500K) to remove organic and inorganic impurities, which is not only time-consuming and energy-intensive but also requires sophisticated surface coating techniques, making them less than ideal for waste graphite recycling. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention proposes a method for the regeneration and repair of graphite anode sheets from waste lithium-ion batteries. This method enables rapid repair of waste graphite in a short time, significantly reducing the cost of waste battery processing. Furthermore, the regeneration and repair method is simple in its steps and does not generate secondary pollution, providing a new approach for the repair and regeneration of anode materials from waste lithium-ion batteries.
[0005] To achieve the above objectives, the present invention provides the following technical solution:
[0006] One of the technical solutions of the present invention:
[0007] A method for regenerating and repairing graphite anode sheets from waste lithium-ion batteries includes the following steps:
[0008] The graphite anode sheets from waste lithium-ion batteries are subjected to ultrasonic treatment, drying, plasma ball milling, and calcination in sequence to finally obtain recycled graphite anode powder.
[0009] The beneficial effects achieved by the above technical solution are as follows: This invention discloses a method for regenerating and repairing graphite anode sheets of waste lithium-ion batteries. Through the combined action of simple plasma discharge and vibration, graphene oxide is generated on the graphite surface, and a carbon coating layer is formed on the graphite surface, thereby increasing the capacity of the graphite. The resulting recycled graphite anode material has electrochemical performance with a higher specific capacity than the theoretical capacity.
[0010] Furthermore, the reaction gas used in the plasma ball milling process is one or more of argon, nitrogen, air, and oxygen.
[0011] Furthermore, the plasma ball milling time is 10-180 min, the discharge frequency is 7-11 kHz, the ball milling speed is 900-1450 r / min, and the ball-to-material ratio is (10-50):1.
[0012] Furthermore, in the roasting step, an inert gas is used as both a protective gas and a carrier gas.
[0013] Furthermore, in the calcination step, the flow rate of the inert gas is 60-250 sccm, the heating rate is 2-10℃ / min, the temperature is 700-1000℃, and then the temperature is maintained at this temperature for 3-6 hours.
[0014] Furthermore, the inert gas is argon or nitrogen.
[0015] Furthermore, the graphite anode sheet is obtained by discharging and dismantling waste lithium-ion battery anode materials.
[0016] The beneficial effects achieved by the above technical solution are as follows: discarded lithium-ion batteries usually still have residual charge. If the residual charge is not released during the processing of lithium-ion batteries, fire and explosion may easily occur during the battery disassembly process. Therefore, before repairing discarded lithium-ion batteries, it is necessary to discharge the discarded lithium-ion batteries first.
[0017] Furthermore, the discharge step specifically involves immersing the waste lithium-ion battery in a 2 mol / L sodium chloride solution for 48 hours for deep discharge.
[0018] Furthermore, the disassembly is done manually, separating the positive electrode, separator, graphite negative electrode, and outer casing.
[0019] The second technical solution of the present invention:
[0020] A regenerated lithium-ion battery negative electrode sheet includes regenerated graphite negative electrode powder prepared by the above-mentioned regeneration and repair method.
[0021] Furthermore, the recycled lithium-ion battery negative electrode also includes conductive carbon and PVDF.
[0022] Furthermore, the mass ratio of the recycled graphite anode powder to conductive carbon and PVDF is 8:1:1.
[0023] Compared with the prior art, the present invention has the following advantages and technical effects:
[0024] 1. The regeneration and repair method of the present invention can achieve rapid repair of waste graphite in a short time, which greatly reduces the cost of waste battery treatment; moreover, the regeneration and repair method has simple steps and does not produce secondary pollution, providing a new approach for the repair and regeneration of waste lithium-ion battery anode materials.
[0025] 2. This invention achieves etching and thinning effects, enabling the formation of a graphene oxide carbon coating layer on the surface of waste graphite, thereby providing additional discharge specific capacity. This results in the performance of the recycled graphite anode material exceeding the theoretical specific capacity (1C = 372 mAh g). -1 ). Attached Figure Description
[0026] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. In the drawings:
[0027] Figure 1 The XRD patterns of the waste graphite anode material and the recycled graphite anode material in Example 1 are shown.
[0028] Figure 2 (a1, a2, a3) are SEM and EDS images of the waste graphite anode material from Example 1; Figure 2 (b1, b2, b3) are the SEM and EDS images of the recycled graphite anode material in Example 1;
[0029] in, Figure 2 a1 and a2 are SEM images of the waste graphite anode material from Example 1; Figure 2 a3 is the EDS spectrum of the waste graphite anode material from Example 1;
[0030] Figure 2 b1 and b2 are SEM images of the recycled graphite anode material from Example 1; Figure 2 b3 is the EDS spectrum of the recycled graphite anode material in Example 1;
[0031] Figure 3 The charge-discharge curves of the waste graphite anode material and the recycled graphite anode material in Example 1 at a rate of 0.2C are shown.
[0032] Figure 4 The graph shows the cycling performance of waste graphite and recycled graphite samples from Example 1 after 220 cycles at a 0.2C rate within a voltage range of 0.01-2.0V.
[0033] Figure 5 Here is a SEM image of the recycled graphite anode material from Example 2;
[0034] Figure 6 The graph shows the cycling performance of the recycled graphite anode material in Example 2 at a rate of 0.2C within a voltage range of 0.01-2.0V.
[0035] Figure 7 Here is a SEM image of the recycled graphite anode material from Example 3;
[0036] Figure 8 The graph shows the cycling performance of the recycled graphite anode material in Example 3 at a rate of 0.2C within a voltage range of 0.01-2.0V.
[0037] Figure 9 Here is a SEM image of the recycled graphite anode material in Comparative Example 1;
[0038] Figure 10 The graph shows the cycling performance of the recycled graphite anode material in Comparative Example 1 at a rate of 0.2C within a voltage range of 0.01-2.0V.
[0039] in, Figure 1-10 In this context, the waste graphite anode material is waste graphite anode powder after ultrasonic drying; the recycled graphite anode material is recycled graphite anode powder obtained after calcination. Detailed Implementation
[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0041] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0042] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0043] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be readily apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0044] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0045] This invention discloses a method for repairing the negative electrode of a spent lithium-ion battery, comprising the following steps:
[0046] (1) The waste lithium-ion battery was immersed in a 2 mol / L sodium chloride solution for 48 hours for deep discharge. Then the battery was disassembled by hand to separate the positive electrode, separator, graphite negative electrode, shell, etc. The graphite negative electrode was cut into pieces and placed in a beaker for ultrasonic treatment to separate the copper foil from the graphite negative electrode material. After drying, the waste graphite negative electrode powder was obtained.
[0047] (2) Place the waste graphite negative electrode powder from step (1) into a plasma ball mill and perform plasma ball milling in different gases;
[0048] (3) The plasma-repaired negative electrode material from step (2) is placed in a tube furnace and calcined to obtain regenerated graphite negative electrode powder.
[0049] In some preferred embodiments, the plasma ball milling reaction gas in step (2) is one or more of argon, nitrogen, air and oxygen.
[0050] In some preferred embodiments, the plasma discharge ball milling time in step (2) is 10-180 min, the discharge frequency is 7-11 kHz, the ball milling speed is 900-1450 r / min, and the ball-to-material ratio is (10-50):1.
[0051] In some preferred embodiments, step (3) of tube furnace roasting uses an inert gas as a protective gas and a carrier gas, and the inert gas is argon or nitrogen.
[0052] In some preferred embodiments, the flow rate of the inert gas in step (3) of the tubular furnace roasting is 60-250 sccm, the heating rate is 2-10℃ / min, the temperature is 700-1000℃, and the processing time is 3-6h.
[0053] All raw materials used in the embodiments of this invention were obtained through commercial purchase.
[0054] The technical solution of the present invention will be further illustrated by the following embodiments.
[0055] Example 1
[0056] A method for repairing the negative electrode of a spent lithium-ion battery includes the following steps:
[0057] (1) The waste lithium-ion battery was immersed in a 2 mol / L sodium chloride solution for 48 hours for deep discharge. Then the battery was disassembled by hand to separate the positive electrode, separator, graphite negative electrode, shell, etc. The graphite negative electrode was cut into pieces and placed in a beaker for ultrasonic treatment to separate the copper foil from the graphite negative electrode material. After drying, the waste graphite negative electrode powder was obtained.
[0058] (2) Place the 5g waste graphite negative electrode powder from step (1) into a plasma ball milling jar and perform plasma discharge and vibration ball milling operations in argon gas; wherein, the discharge ball milling time is 60min, the discharge frequency is 10KHz, the ball milling speed is 1300r / min, and the ball-to-material ratio is 20:1.
[0059] (3) The plasma-repaired negative electrode material from step (2) was placed in a tube furnace for calcination. The argon flow rate was 200 sccm, the heating rate was 5℃ / min, the temperature was 800℃, and the treatment time was 3h to obtain regenerated graphite negative electrode powder. The regenerated graphite negative electrode powder was uniformly mixed with conductive carbon and PVDF in a mass ratio of 8:1:1 and coated onto copper foil to prepare a negative electrode sheet. The sheet was then assembled into a CR2025 coin cell in an argon glove box, and its electrochemical performance was tested.
[0060] Figure 1 The XRD patterns (scanning speed 10° / min, scanning angle 10-90°) of the waste graphite anode material and the recycled anode material in Example 1 are shown below. Figure 1It can be seen that two of the materials match well with the graphite standard PDF card, without any impurity peaks. Notably, compared with waste graphite, the (002) diffraction peak intensity of recycled graphite is significantly sharper and higher. This indicates that the plasma discharge vibration method yields recycled graphite with a better crystal structure.
[0061] Figure 2 The images shown are SEM and EDS images of the waste graphite anode material and the recycled graphite anode material from Example 1. Figure 2 a1 and a2 are SEM images of the waste graphite negative electrode of Example 1. Due to long-term charge-discharge cycles, its surface is relatively rough, with many aggregated and peeled graphite layers, which require appropriate repair to restore its structure and capacity. Figure 2 b1 and b2 are SEM images of the recycled graphite material in Example 1. It can be seen that the material after plasma discharge vibration treatment becomes a translucent sheet, and graphene oxide is formed on the graphite layer on the surface. Figure 2 Image a3 is the EDS image of the waste graphite negative electrode from Example 1. The waste graphite contains abundant O, F, and P elements, indicating that the aggregated material mainly consists of residual PVDF, SEI film, and electrolyte. Figure 2 b3 is the EDS diagram of the recycled graphite material in Example 1. The content of O, F and P elements in the recycled graphite is reduced, which means that some impurities can be effectively removed in the plasma discharge and vibratory ball milling methods.
[0062] Figure 3 The first charge-discharge curves of the waste graphite and recycled graphite samples in Example 1 at 0.2C are shown. Figure 4 The waste graphite and recycled graphite samples in Example 1 were subjected to a voltage range of 0.01-2.0V and a voltage of 0.2C (1C = 372mAh g). -1 Cycling performance graph at 220 cycles under a certain magnification, from Figure 4 The results show that the first-cycle discharge specific capacity of the waste graphite anode material is only 261.7 mAh g. -1 The repaired graphite anode material has a capacity of 419.7 mAh g. -1 The high capacity, with a discharge specific capacity greater than the theoretical specific capacity, is due to the combined effect of plasma discharge and vibration, which forms an oxide graphene interface on the graphite surface, providing some additional capacity.
[0063] Example 2
[0064] A method for repairing the negative electrode of a spent lithium-ion battery includes the following steps:
[0065] (1) The waste lithium-ion battery was immersed in a 2 mol / L sodium chloride solution for 48 hours for deep discharge. Then the battery was disassembled by hand to separate the positive electrode, separator, graphite negative electrode, shell, etc. The graphite negative electrode was cut into pieces and placed in a beaker for ultrasonic treatment to separate the copper foil from the graphite negative electrode material. After drying, the waste graphite negative electrode powder was obtained.
[0066] (2) Place the 5g waste graphite negative electrode powder from step (1) into a plasma ball milling jar and perform plasma discharge and vibration ball milling operations in nitrogen gas; the discharge ball milling time is 30min, the discharge frequency is 10KHz, the ball milling speed is 1400r / min, and the ball-to-material ratio is 30:1.
[0067] (3) The plasma-repaired negative electrode material from step (2) was placed in a tube furnace for calcination. The nitrogen flow rate was 250 sccm, the heating rate was 10℃ / min, the temperature was 900℃, and the treatment time was 5h to obtain regenerated graphite negative electrode powder. The regenerated graphite negative electrode powder was uniformly mixed with conductive carbon and PVDF at a mass ratio of 8:1:1 and coated onto copper foil to prepare a negative electrode sheet. The negative electrode sheet was assembled into a CR2025 coin cell in an argon glove box, and its electrochemical performance was tested.
[0068] Figure 5 This is a SEM image of the recycled graphite anode material from Example 2. As can be seen from the image, the recycled material after plasma ball milling exhibits a semi-transparent, sheet-like structure.
[0069] Figure 6 The graph shows the performance of the recycled graphite sample in Example 2 after 100 cycles at 0.2C. It can be seen that the first-cycle discharge specific capacity of the recycled graphite anode material is 438.1 mAh g. -1 After 100 cycles, the discharge specific capacity is 369.5 mAh g. -1 .
[0070] Example 3
[0071] A method for repairing the negative electrode of a spent lithium-ion battery includes the following steps:
[0072] (1) The waste lithium-ion battery was immersed in a 2 mol / L sodium chloride solution for 48 hours for deep discharge. Then the battery was disassembled by hand to separate the positive electrode, separator, graphite negative electrode, shell, etc. The graphite negative electrode was cut into pieces and placed in a beaker for ultrasonic treatment to separate the copper foil from the graphite negative electrode material. After drying, the waste graphite negative electrode powder was obtained.
[0073] (2) Place the 5g waste graphite negative electrode powder from step (1) into a plasma ball milling jar and perform plasma discharge and vibration ball milling operations in nitrogen gas; the discharge ball milling time is 10min, the discharge frequency is 10KHz, the ball milling speed is 1450r / min, and the ball-to-material ratio is 50:1.
[0074] (3) The plasma-repaired negative electrode material from step (2) was placed in a tube furnace for calcination. The nitrogen flow rate was 150 sccm, the heating rate was 2℃ / min, the temperature was 1000℃, and the treatment time was 6h to obtain regenerated graphite negative electrode powder. The regenerated graphite negative electrode powder was uniformly mixed with conductive carbon and PVDF in a mass ratio of 8:1:1 and coated onto copper foil to prepare a negative electrode sheet. The sheet was assembled into a CR2025 coin cell in an argon glove box, and its electrochemical performance was tested.
[0075] Figure 7 This is a SEM image of the regenerated graphite anode material after plasma ball milling in Example 3. It can be seen that the regenerated material has a semi-transparent, sheet-like morphology.
[0076] Figure 8 The graph shows the cycling performance of the recycled graphite sample in Example 3 after 100 cycles at 0.2C. It can be seen that the first-cycle discharge specific capacity of the recycled graphite anode material is 413.6 mAh g. -1 After 100 cycles, the discharge specific capacity is 401.9 mAh g. -1 The capacity retention rate was 97.1%.
[0077] Comparative Example 1
[0078] Except for step (2), in which the traditional acid leaching regeneration method is used instead of the plasma ball milling method, the sulfuric acid concentration is 4 mol / L, the solid-liquid ratio is 1:3, the magnetic stirring speed is set to 800 rpm, and the leaching time is set to 6 h, the rest is the same as in Example 1.
[0079] Figure 9 The image shows a SEM image of the graphite anode material obtained by the traditional acid leaching regeneration method in Comparative Example 1. The image shows that the regenerated material has a blocky morphology.
[0080] Figure 10 The graph shows the cycling performance of the recycled graphite sample in Comparative Example 1 at a rate of 0.2C, with an initial discharge specific capacity of 366.1 mAh g. -1 After 100 cycles, the discharge specific capacity is 340 mAh g. -1 The capacity retention rate was 92.8%. This comparative example shows that the traditional acid leaching method is not only time-consuming and generates secondary pollution, but also the electrochemical performance of the recycled graphite anode material does not reach the level of commercial graphite.
[0081] The above are merely preferred embodiments of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.
Claims
1. A method for regenerating and repairing graphite anode sheets from waste lithium-ion batteries, characterized in that, Includes the following steps: The graphite anode sheets from waste lithium-ion batteries are subjected to ultrasonic treatment, drying, plasma ball milling, and calcination in sequence to finally obtain recycled graphite anode powder. The plasma ball milling time is 10-180 min, the discharge frequency is 7-11 kHz, the ball milling speed is 900-1450 r / min, and the ball-to-material ratio is (10-50):1; Inert gas is used as both protective gas and carrier gas during the roasting process; During the calcination process, the flow rate of the inert gas is 60-250 sccm, the heating rate is 2-10℃ / min, the temperature is raised to 700-1000℃, and the temperature is held at this temperature for 3-6 hours.
2. The method for regenerating and repairing graphite negative electrode sheets of waste lithium-ion batteries according to claim 1, characterized in that, The reaction gas used in the plasma discharge and vibratory ball milling process is one or more of argon, nitrogen, air and oxygen.
3. The method for regenerating and repairing graphite negative electrode sheets from waste lithium-ion batteries according to claim 1, characterized in that, The inert gas is argon or nitrogen.
4. The method for regenerating and repairing graphite negative electrode sheets of waste lithium-ion batteries according to claim 1, characterized in that, The graphite anode sheet is obtained by discharging and dismantling waste lithium-ion battery anode materials.
5. The method for regenerating and repairing graphite negative electrode sheets of waste lithium-ion batteries according to claim 4, characterized in that, The discharge step specifically involves immersing the waste lithium-ion battery in a 2 mol / L sodium chloride solution for 48 hours for deep discharge.
6. A regenerated lithium-ion battery negative electrode sheet, characterized in that, The regenerated graphite anode powder prepared by the regeneration and repair method according to any one of claims 1-5.
7. The regenerated lithium-ion battery negative electrode sheet according to claim 6, characterized in that, The regenerated lithium-ion battery negative electrode also includes conductive carbon and PVDF.
Citation Information
Patent Citations
Application method of cold field plasma discharge assisted high energy ball milled powder and plasma assisted high energy ball milling device
CN104549658A
Repairing modifying method of cathode waste material of waste lithium ion battery
CN105356001A