A method for preparing a cellulose acetate hydrophobic gas permeable composite membrane
By scraping a hydrophobic functional layer onto a cellulose acetate nanofiber substrate and performing an urethane reaction, a porous structure is formed through phase inversion. This solves the problem of insufficient hydrophobic and air-permeable properties of cellulose acetate separation membranes, achieving stable hydrophobic characteristics and efficient mass transfer performance of the composite membrane, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202410389388.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-02
AI Technical Summary
Existing cellulose acetate separation membranes have shortcomings in terms of hydrophobic and air-permeable properties, which limits their application in membrane distillation and unidirectional moisture conduction.
A hydrophobic and breathable composite membrane of cellulose acetate was prepared by scraping a hydrophobic functional layer onto a cellulose acetate nanofiber substrate and performing an urethane reaction, which combined with phase transformation to form a porous structure.
The hydrophobic and air-permeable properties of cellulose acetate separation membranes have been achieved. The process is simple and low-cost, making it suitable for industrial application. Furthermore, the functional layer and the base membrane layer have good compatibility, which enhances the mass transfer potential of the separation membrane.
Smart Images

Figure CN118105844B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of green fiber composite membrane technology, specifically a method for preparing a cellulose acetate hydrophobic and breathable composite membrane. Background Technology
[0002] Membrane separation technology is widely used in environmental purification and medical and health fields, and has the advantages of simple operation, low cost, and environmental friendliness. In recent years, research on separation membranes has gradually expanded from traditional fields to new fields such as membrane distillation and unidirectional moisture conduction. For example, membrane distillation technology, represented by hydrophobic and breathable membranes, has shown excellent performance characteristics in the upgrading and reuse of high-concentration chemical wastewater and biomass fiber degumming wastewater.
[0003] Cellulose acetate (CA) is one of the earliest developed and most widely used membrane-forming polymer materials. It is processed into different types of membrane modules and applied in microfiltration, ultrafiltration, nanofiltration, reverse osmosis, and other forms of membrane separation processes. At the same time, CA's membrane-forming properties and biomass attributes have made it a preferred polymer raw material for membrane products with emerging demands. Compared with petrochemical polymers such as polyvinylidene fluoride, which are commonly used in hydrophobic and breathable membranes, CA has significant cost and environmental advantages.
[0004] However, cellulose acetate (CA) belongs to the category of hydrophilic polymers. Therefore, CA separation membranes need to be constructed with hydrophobic and breathable properties to achieve applications such as membrane distillation, unidirectional moisture conduction, and others. Currently, research on the modification of the hydrophobic and breathable properties of CA and its separation membrane products has received widespread attention from academia and engineering. For example, application number 201610566301.X discloses a water-based paint containing superhydrophobic composite cellulose acetate nanofibers for wooden handicrafts and its preparation method. This method improves the hydrophobic properties of the nanofiber membrane by fluorinating the breathable cellulose acetate nanofiber membrane with fluorinated polysiloxane. Application number 201410343622.4 discloses a preparation method and application of hydrophobic polymer-modified cellulose acetate. This method utilizes free radical polymerization to obtain a hydrophobic polymer and complete the hydrophobic modification of cellulose acetate. Application No. 202010275358.0 discloses a highly hydrophobic cellulose acetate aerogel and its preparation method. This method utilizes diisocyanate as a crosslinking agent to combine fluorinated and / or silane-based hydrophobic agents with cellulose acetate, followed by supercritical drying to produce a hydrophobic aerogel. These studies have achieved the construction of hydrophobic cellulose acetate and its profiles through different technologies; however, the use of fluorinated hydrophobic compounds and the relatively complex preparation process limit its widespread application.
[0005] Based on this, the focus has become on developing and preparing a cellulose acetate separation membrane with both hydrophobic and permeable properties through chemical reactions to meet its applications in membrane distillation, unidirectional moisture conduction, and other fields, and establishing a simple and stable new process. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the technical problem this invention aims to solve is to provide a method for preparing a cellulose acetate hydrophobic and breathable composite membrane.
[0007] The technical solution of the present invention to solve the aforementioned technical problem is to provide a method for preparing a cellulose acetate hydrophobic and breathable composite membrane, characterized in that the method includes the following steps:
[0008] Step 1: Dissolve cellulose acetate and pore-forming agent in a solvent to prepare a homogeneous reaction solution;
[0009] The pore-forming agent is a water-soluble solid substance without active proton groups; the solvent is an organic solvent that is miscible with water and does not contain active proton groups.
[0010] Step 2: Add MTIS to the homogeneous reaction solution, then add DBTDL as a catalyst, and carry out the esterification reaction until no more bubbles are generated. After standing to remove bubbles, a homogeneous casting solution is obtained.
[0011] Step 3: Scrape the casting solution into a flat liquid film;
[0012] Step 4: Evenly spread the cellulose acetate nanofiber base membrane on the flat liquid membrane to construct the flat composite liquid membrane;
[0013] Step 5: Place the flat composite liquid membrane in a coagulation bath to solidify and form a flat composite membrane; then immerse it in deionized water until the pore-forming agent is completely removed, then wash it with deionized water to remove the residual solvent or impurities on the surface of the flat composite membrane, and then freeze-dry it to completely remove the moisture inside and on the surface of the composite membrane to obtain a hydrophobic and breathable cellulose acetate composite membrane.
[0014] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0015] (1) Based on the in-situ hydrophobic modification of cellulose acetate casting solution, this invention introduces a hydrophobic functional layer of cellulose acetate on the surface of nanofiber base membrane by reverse deposition surface coating technology, and at the same time utilizes phase transformation to form a porous structure to obtain a hydrophobic and breathable composite membrane of cellulose acetate.
[0016] (2) This method has simple operation process, mild reaction conditions, low material and processing costs, and is easy to implement, making it suitable for large-scale preparation and industrial promotion.
[0017] (3) In this invention, a m-tolyl hydrophobic group is introduced into the cellulose acetate molecule through an urethane reaction, and the hydroxyl group of cellulose acetate is transformed into a m-tolyl urethane group. The hydrophobic group is firmly connected through the bonding of chemical bonds, thereby constructing a functional layer with stable hydrophobic properties in the composite membrane.
[0018] (4) Unlike the process of “direct coating + phase transformation” on nanofiber base film, the present invention first scrapes the hydrophobic functional layer into a flat liquid film composed of hydrophobic material, then evenly lays the nanofiber base film on the hydrophobic flat liquid film, and then the combination is phase transformed together to complete the preparation of the composite film.
[0019] (5) In this invention, cellulose acetate nanofiber membrane is selected as the base membrane. The base membrane layer and the functional layer belong to the same series of polymers and have good compatibility. The nanofiber helps to improve the mass transfer potential of the separation membrane.
[0020] (6) The composite membrane prepared by this invention uses a cellulose acetate nanofiber membrane as the base layer and a hydrophobic and breathable flat liquid membrane as the functional layer. The two are combined to form a functional layer with hydrophobic properties and porous breathability on the surface of the base layer. The hydrophobic properties of the functional layer are achieved by introducing hydrophobic groups through an esterification reaction; the breathability of the functional layer is achieved by using a phase inversion membrane process to form a porous structure under the flat composite liquid membrane, thereby constructing porous breathability. Attached Figure Description
[0021] Figure 1 This is a process flow diagram of the method of the present invention;
[0022] Figure 2 The water contact angle diagrams are shown for the hydrophobic and breathable composite membranes of cellulose acetate prepared in Examples 1-5 of the present invention and the nanofiber membrane of cellulose triacetate prepared in Comparative Example 1.
[0023] Figure 3 XPS image of the functional layer in the cellulose acetate hydrophobic and breathable composite membrane prepared in Example 3 of this invention;
[0024] Figure 4 This is a SEM image of the functional layer in the cellulose acetate hydrophobic and breathable composite membrane prepared in Example 3 of the present invention.
[0025] Figure 5 This is a SEM image of the base film layer in the cellulose acetate hydrophobic and breathable composite membrane prepared in Example 3 of the present invention.
[0026] Figure 6 The images show the FTIR images of the functional layer and the base film layer in the cellulose acetate hydrophobic and breathable composite membrane prepared in Example 5 of this invention.
[0027] Figure 7The image shows the FTIR of the cellulose triacetate nanofiber membrane prepared in Comparative Example 1 of this invention.
[0028] Figure 8 XPS image of the cellulose triacetate nanofiber membrane prepared in Comparative Example 1 of this invention;
[0029] Figure 9 This is a SEM image of the cellulose triacetate nanofiber membrane prepared in Comparative Example 1 of this invention. Detailed Implementation
[0030] Specific embodiments of the present invention are given below. These specific embodiments are only used to further illustrate the present invention in detail and do not limit the scope of protection of the claims of the present invention.
[0031] This invention provides a method for preparing a cellulose acetate hydrophobic and breathable composite membrane (hereinafter referred to as the method), characterized in that the method includes the following steps:
[0032] Step 1: Dissolve cellulose acetate and pore-forming agent in a solvent to prepare a homogeneous reaction solution;
[0033] Preferably, in step 1, the cellulose acetate is cellulose acetate with an acetyl substitution degree of less than 2.5.
[0034] Preferably, in step 1, the pore-forming agent is a water-soluble solid substance that does not contain active proton groups, including polyvinylpyrrolidone (PVP), polyethylene oxide (PEO), polyquaternary ammonium salts, surfactants, organic carboxylates, and water-soluble salt compounds; the surfactants include sodium dodecyl sulfate and potassium dodecyl sulfate; the organic carboxylates include sodium acetate and calcium oxalate; and the water-soluble salt compounds include calcium chloride, potassium chloride, and sodium sulfate.
[0035] Preferably, in step 1, the solvent is an organic solvent that is miscible with water and does not contain active proton groups, specifically N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and 1,4-dioxane.
[0036] Preferably, in step 1, the homogeneous reaction solution contains 10-20 wt% cellulose acetate and 1-5 wt% porogen.
[0037] Step 2: Add MTIS (m-toluene isocyanate) to the homogeneous reaction solution, and then add DBTDL (dibutyl dilaurate) as a catalyst to carry out the amination reaction until no more bubbles are generated. After the reaction is completed, the homogeneous casting solution is obtained after standing and degassing.
[0038] Preferably, in step 2, MTIS is added dropwise to the homogeneous reaction solution to avoid the highly reactive exothermic reaction between isocyanate groups and hydroxyl groups, which could lead to excessively high local temperatures in the solution and affect the casting solution system.
[0039] Preferably, in step 2, the ratio of the amount of MTIS to the amount of hydroxyl groups in cellulose acetate is 1 to 1.5:1; DBTDL accounts for 0.1 to 1 wt% of the total casting solution.
[0040] Preferably, in step 2, the addition rate of MTIS is controlled to maintain the system temperature at the urethane reaction temperature, thus avoiding the side reaction of MTIS self-polymerization due to excessively high temperature. The urethane reaction temperature is at most 40°C (preferably 0–40°C, more preferably 15–35°C, even more preferably 20–30°C), and the reaction time is 1–5 h (preferably 2–4 h).
[0041] Preferably, step 2 is carried out under stirring conditions.
[0042] Step 3: In an environment with a temperature of 15-30℃ and a humidity of 25%-60%, the casting solution is scraped into a flat liquid film of a certain thickness.
[0043] Preferably, in step 3, the thickness of the flat liquid film is 50-400 μm, more preferably 100-300 μm. Taking into account factors such as bonding, hydrophobicity, and air permeability, hydrophobic functional flat liquid film layers of different thicknesses are constructed.
[0044] Step 4: Evenly spread the cellulose acetate nanofiber base membrane on the flat liquid membrane to construct a flat composite liquid membrane with an asymmetric hydrophilic and hydrophobic structure.
[0045] Preferably, in step 4, the cellulose acetate nanofiber substrate membrane is an electrospun cellulose acetate nanofiber membrane, a solution-jet spun cellulose acetate microfiber membrane, or a cellulose acetate nanofiber nonwoven material.
[0046] Step 5: Place the flat composite liquid membrane in a coagulation bath to solidify and form a flat composite membrane; then immerse it in deionized water until the pore-forming agent is completely removed, then wash it with deionized water to remove the residual solvent or impurities on the surface of the flat composite membrane, and then freeze-dry it to completely remove the moisture inside and on the surface of the composite membrane to obtain a hydrophobic and breathable cellulose acetate composite membrane.
[0047] Preferably, in step 5, the coagulation bath uses deionized water at 10–30°C.
[0048] Preferably, in step 5, the immersion time in deionized water is not less than 12 hours.
[0049] Preferably, in step 5, the surface of the flat composite film is washed 2-3 times with deionized water to remove residual solvents or impurities.
[0050] Preferably, in step 5, the freeze-drying process is: freeze-drying in an environment with a temperature < -30℃ and a vacuum degree < 100Pa for 20 to 30 hours (preferably 24 hours).
[0051] The structure, morphology, and performance testing methods of the embodiments and comparative examples are as follows:
[0052] (a) Structural testing: The product was analyzed using Fourier transform infrared spectroscopy (FTIR), with a scanning range of 4000-500 cm⁻¹. -1 The scanning resolution is 4cm. -1 The scan was performed 32 times. The products were tested and analyzed using X-ray photoelectron spectroscopy (XPS) with monochromatic Al-Kα X-rays as the light source (hυ=1486.6V). The product binding energy was measured in the range of 0~1000eV.
[0053] (b) Morphology test: The morphology of the product was observed using a scanning electron microscope (SEM) to obtain SEM images with a magnification of 2000×.
[0054] (c) Performance Testing: The water contact angle (WCA) of the product was measured at room temperature using a contact angle meter. A 5 μL drop of deionized water was placed on the product surface, and the WCA value was measured after it stabilized. The air permeability of the product was tested using a fully automated air permeability meter, with a test pressure difference of 200 Pa and a test area of 20 cm². 2 .
[0055] Example 1
[0056] (1) Dissolve 6g of cellulose acetate with an acetyl substitution degree of 2.45 and 1.2g of PVP in 32.80g of DMF and stir until the solid mixture is completely dissolved into a homogeneous reaction solution.
[0057] (2) At room temperature, under stirring at 200 rpm, 2.5 g of MTIS was added dropwise to the homogeneous reaction solution, and then 0.10 g of DBTDL was added dropwise. The amination reaction was carried out for 2 hours. After standing and degassing, a homogeneous casting solution was obtained.
[0058] (3) In an environment with a temperature of 25℃ and a humidity of 40%, a 100μm doctor blade is selected to scrape the casting liquid into a flat liquid film with a thickness of 100μm.
[0059] (4) The electrospun cellulose triacetate nanofiber membrane is evenly spread on the flat liquid membrane to form a flat composite liquid membrane.
[0060] The specific steps for preparing cellulose triacetate nanofiber membranes by electrospinning are as follows: cellulose triacetate (CTA) with a higher degree of acetylation is selected as the spinning polymer; the mass fraction of cellulose triacetate in the spinning solution is 5%, dissolved in a mixed solvent composed of dichloromethane / N,N-dimethylformamide at a mass ratio of 8:1; the spinning solution is spun at a feed rate of 3.5 mL / h under conditions of 12 kV spinning voltage and 1 cm horizontal receiving distance to form nanofibers, which are then collected on the surface of a roller to form a cellulose triacetate nanofiber membrane, which is then dried in an oven at 50℃ to constant weight.
[0061] (5) The flat composite liquid membrane is immersed in a deionized water coagulation bath at 25°C to solidify and form a flat composite membrane; then it is transferred to deionized water at 25°C for 24 hours to fully remove the pore-forming agent, and then washed three times with deionized water to remove the residual solvent or impurities on the surface of the flat composite membrane. The flat composite membrane is then placed in a freeze dryer at -40°C and a vacuum of 10Pa for 24 hours to completely remove the moisture inside and on the surface of the composite membrane, thus obtaining a hydrophobic and breathable cellulose acetate composite membrane.
[0062] The composite membrane was tested and found to have a WCA value of 104.1°, exhibiting hydrophobic properties. The air permeability of the composite membrane was 0.890 mm / s.
[0063] Example 2
[0064] This embodiment is the same as that in embodiment 1, except that the thickness of the scraper and the thickness of the flat liquid film in step (3) are both 150 μm.
[0065] The composite membrane was tested and found to have a WCA value of 95.6°, exhibiting hydrophobic properties. The air permeability of the composite membrane was 0.853 mm / s.
[0066] Example 3
[0067] This embodiment is the same as that in embodiment 1, except that the thickness of the scraper and the thickness of the flat liquid film in step (3) are both 200 μm.
[0068] The composite membrane was tested and found to have a WCA value of 114.8°, exhibiting hydrophobic properties. The air permeability of the composite membrane was 1.079 mm / s.
[0069] Depend on Figure 3 It can be seen that the characteristic peak of N element in the spectrum proves that the hydrophobic modification is complete.
[0070] Depend on Figure 4 As can be seen, the functional layer exhibits a typical dense microporous structure, which facilitates the transfer and transport of gas molecules.
[0071] Depend on Figure 5It can be seen that the base film layer exhibits a typical nanofiber structure, indicating that the composite film exhibits an asymmetric structure.
[0072] Example 4
[0073] This embodiment is the same as that in embodiment 1, except that the thickness of the scraper and the thickness of the flat liquid film in step (3) are both 250 μm.
[0074] The composite membrane was tested and found to have a WCA value of 101.3°, exhibiting hydrophobic properties. The air permeability of the composite membrane was 0.899 mm / s.
[0075] Example 5
[0076] This embodiment is the same as that in embodiment 1, except that the thickness of the scraper and the thickness of the flat liquid film in step (3) are both 300 μm.
[0077] The composite membrane was tested and found to have a WCA value of 103.3°, exhibiting hydrophobic properties. The air permeability of the composite membrane was 0.871 mm / s.
[0078] Depend on Figure 6 As can be seen, the NH characteristic peak in the functional layer confirms the completion of the hydrophobic modification reaction via urethane esterification. The base film layer exhibits typical structural characteristic peaks of cellulose acetate, indicating that the modification process does not affect or alter the chemical structure of the base film.
[0079] Comparative Example 1
[0080] The comparative example selected the cellulose triacetate nanofiber membrane prepared in step (4) of Example 1.
[0081] The cellulose triacetate nanofiber membrane was tested and found to have a WCA value of 73.9°, exhibiting hydrophilic properties. The air permeability of the cellulose triacetate nanofiber membrane was 75.22 mm / s.
[0082] Depend on Figure 2 It can be seen that the composite membranes prepared in Examples 1-5 exhibit hydrophobic properties, while the triacetate cellulose nanofiber membrane prepared in Comparative Example 1 exhibits hydrophilic properties.
[0083] Depend on Figure 7 It can be seen that 1740cm -1 The C=O characteristic peak at the point indicates that the polymer belongs to the cellulose acetate series.
[0084] Depend on Figure 8 It can be seen that the characteristic peaks of C and O elements in the spectrum prove that the fiber membrane is spun from cellulose acetate and does not contain other solvents or components.
[0085] Depend on Figure 9It can be seen that the cellulose triacetate nanofibers are randomly stacked and arranged to form a large pore structure, which is significantly different from the dense surface microporous structure of the functional layer of the composite membrane.
[0086] Any aspects not covered in this invention are applicable to existing technologies.
Claims
1. A method for preparing a cellulose acetate hydrophobic and breathable composite membrane, characterized in that, The method includes the following steps: Step 1: Dissolve cellulose acetate and pore-forming agent in a solvent to prepare a homogeneous reaction solution; Cellulose acetate is used with an acetyl substitution degree of less than 2.5; the pore-forming agent is a water-soluble solid substance without active proton groups; the solvent is an organic solvent that is miscible with water and does not contain active proton groups. Step 2: Add m-toluene isocyanate MTIS to the homogeneous reaction solution, and then add dibutyl dilaurate DBTDL as a catalyst to carry out the esterification reaction until no more bubbles are generated. After standing to remove bubbles, a homogeneous casting solution is obtained. Step 3: Scrape the casting solution into a flat liquid film; Step 4: Evenly spread the cellulose acetate nanofiber base membrane on the flat liquid membrane to form a flat composite liquid membrane; Step 5: Place the flat composite liquid membrane in a coagulation bath to solidify and form a flat composite membrane; then immerse it in deionized water until the pore-forming agent is completely removed, then wash it with deionized water to remove the residual solvent or impurities on the surface of the flat composite membrane, and then freeze-dry it to completely remove the moisture inside and on the surface of the composite membrane to obtain a hydrophobic and breathable cellulose acetate composite membrane.
2. The method for preparing the cellulose acetate hydrophobic and breathable composite membrane according to claim 1, characterized in that, In step 1, the pore-forming agent includes polyvinylpyrrolidone, polyethylene oxide, polyquaternary ammonium salt, surfactant, organic carboxylate, and water-soluble salt compound; the surfactant includes sodium dodecyl sulfate and potassium dodecyl sulfate; the organic carboxylate includes sodium acetate and calcium oxalate; and the water-soluble salt compound includes calcium chloride, potassium chloride, and sodium sulfate. The solvents are N,N-dimethylformamide, N,N-dimethylacetamide and 1,4-dioxane.
3. The method for preparing the cellulose acetate hydrophobic and breathable composite membrane according to claim 1, characterized in that, In step 1, the homogeneous reaction solution contains 10-20 wt% cellulose acetate and 1-5 wt% porogen.
4. The method for preparing the cellulose acetate hydrophobic and breathable composite membrane according to claim 1, characterized in that, In step 2, the ratio of the amount of MTIS to the amount of hydroxyl groups in cellulose acetate is 1~1.5:1; DBTDL accounts for 0.1~1wt% of the total casting solution mass.
5. The method for preparing the cellulose acetate hydrophobic and breathable composite membrane according to claim 1, characterized in that, In step 2, the temperature of the esterification reaction is at most 40°C, and the reaction time is 1~5h.
6. The method for preparing the cellulose acetate hydrophobic and breathable composite membrane according to claim 1, characterized in that, In step 2, MTIS is added dropwise to the homogeneous reaction solution; the entire step 2 is carried out under stirring conditions.
7. The method for preparing the cellulose acetate hydrophobic and breathable composite membrane according to claim 1, characterized in that, In step 3, the ambient temperature of the film-scraping environment is 15~30℃ and the humidity is 25%~60%; the thickness of the flat liquid film is 50~400μm.
8. The method for preparing the cellulose acetate hydrophobic and breathable composite membrane according to claim 1, characterized in that, In step 4, the cellulose acetate nanofiber substrate membrane is an electrospun cellulose acetate nanofiber membrane, a solution-jet spun cellulose acetate microfiber membrane, or a cellulose acetate nanofiber nonwoven material.
9. The method for preparing the cellulose acetate hydrophobic and breathable composite membrane according to claim 1, characterized in that, In step 5, the coagulation bath uses deionized water at 10~30℃; the immersion time in deionized water is not less than 12 hours.
10. The method for preparing the cellulose acetate hydrophobic and breathable composite membrane according to claim 1, characterized in that, In step 5, the freeze-drying process is as follows: freeze-dry in an environment with a temperature of <-30℃ and a vacuum degree of <100Pa for 20~30h.
Citation Information
Patent Citations
Preparation method and use of hydrophobic polymer-modified cellulose acetate
CN104130355A
Water paint containing super-hydrophobic composite cellulose acetate nanofibers for wooden crafts and preparation method of water paint
CN106118301A
High-hydrophobicity cellulose acetate aerogel and preparation method thereof
CN111303477A
Preparation method for cellulose acetate forward osmosis membrane
CN105561808A
Method and apparatus for primary shaping composite or modified hollow fibre membrane
CN1552507A