A method for improving the separation performance of CO2 by using topological molecular sieve (ZSM-5) in mixed matrix membranes
By introducing a topological molecular sieve (ZSM-5) into a mixed matrix membrane and modifying it with sulfur/molybdenum, the problems of insufficient permeability and selectivity of the mixed matrix membrane in CO₂/N₂ separation were solved, achieving high performance and low cost CO₂ separation.
Patent Information
- Application Number
- CN202410447622.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-15
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-15
AI Technical Summary
Existing hybrid matrix membranes exhibit low permeability and selectivity in CO₂/N₂ separation, and MOF materials are expensive, making it difficult to achieve a combination of high performance and low cost.
A topological molecular sieve (ZSM-5) was used as a filler and blended with Pebax-1657. Molecular sieve material with CO₂ adsorption performance was introduced through blending and then sulfur/molybdenum modification was performed to form a mixed matrix membrane.
This method improves the CO₂ permeation performance and selectivity of the mixed matrix membrane, achieving high CO₂/N₂ separation performance at a relatively low cost and in line with an environmentally friendly preparation process.
Smart Images

Figure BDA0004791563050000041 
Figure BDA0004791563050000042 
Figure BDA0004791563050000101
Abstract
Description
Technical Field
[0001] This invention belongs to the field of gas separation technology, specifically relating to a method for improving the CO2 separation performance of a mixed matrix membrane using a topological molecular sieve (ZSM-5). Background Technology
[0002] Since the Second Industrial Revolution, human utilization of natural gas and oil has increased significantly. While this has promoted economic development to some extent, CO2 emissions have also increased year by year, contributing to the greenhouse effect and causing a series of environmental problems such as rising sea levels and melting glaciers. Meanwhile, excessive CO2 emissions have attracted global attention, and addressing the resulting environmental problems requires the joint efforts of all countries. With the over-exploitation of non-renewable resources and the depletion of fossil fuels, CO2, as an existing and abundant C1 resource on Earth, is inexpensive, non-toxic, and renewable. Chemical products synthesized using CO2 as a raw material are environmentally friendly and biodegradable. Currently, the efficient utilization of CO2 has attracted widespread attention from various countries.
[0003] Compared to traditional gas separation technologies, membrane separation technology offers advantages such as ease of operation, low energy consumption, and no pollution, and is considered the most promising third-generation separation technology, attracting widespread attention. Among numerous membrane materials, organic membranes have been extensively studied due to their low cost, availability, and ability to be fabricated over large areas. However, these materials struggle to overcome the trade-off between permeability and selectivity, typically limiting their performance below the Robeson upper limit. Inorganic membranes, with their excellent separation performance, thermal stability, and chemical stability, have always been a hot topic in membrane technology research. However, their high cost and fragility hinder further development. To address these issues, researchers have attempted to combine the low cost and ease of fabrication of polymer membranes with the high performance of inorganic membranes, thereby preparing hybrid matrix membranes with superior performance.
[0004] Researchers Maleh et al. synthesized ZIF-67@ZIF-L(Zn) nanoparticles using in-situ heteroepitaxialization. In a Pebax-1657 mixed matrix membrane, they exhibited optimal separation performance at 10 bar and 2 wt.% filler, with a CO2 permeation performance of 72.9 Barrer and a CO2 / N2 selectivity of 102.9.
[0005] Researcher Dai Yan [2]Pebax-1657 was selected as the polymer matrix and ZIF-93 as the inorganic filler. ZIF-93, rich in aldehyde groups, provides CO2 transport channels, facilitating the separation of CO2 in the CO2 / N2 system. The hybrid matrix membrane achieved a CO2 permeation performance (PCO2) of 55.98-85.37 Barrer and a CO2 / N2 selectivity of 58.13-70.84.
[0006] However, the CO2 / N2 separation performance of the hybrid matrix membranes prepared from MOF materials currently studied has not reached the ideal state, and MOFs are relatively expensive. Therefore, it is a challenging task to study an inexpensive inorganic material suitable for the field of gas separation, and to prepare a hybrid matrix membrane with high selectivity and high permeability will be another new challenge. Summary of the Invention
[0007] In view of the above-described background technology, this invention proposes a method for improving the CO2 separation performance of a mixed matrix membrane using a topological molecular sieve (ZSM-5). Specifically, the method involves preparing a mixed matrix membrane for CO2 separation using ZSM-5 as the packing material and Pebax-1657 as the matrix. By introducing a molecular sieve material with CO2 adsorption properties through blending, the problem of low permeability and selectivity of the membrane material for CO2 / N2 is solved.
[0008] The technical solution of the present invention:
[0009] A method for improving the CO2 separation performance of a mixed matrix membrane using a topological molecular sieve (ZSM-5) is characterized by comprising the following steps:
[0010] (1) Preparation of Pebax-1657 solution:
[0011] Place 93-137 parts of Pebax-1657 and 3200-4200 parts of ethanol / water in a flask and stir magnetically for 2.5-5 hours while maintaining a certain temperature to obtain a Pebax solution of uniform concentration.
[0012] (2) Preparation method of pure ZSM-5 filler:
[0013] Weigh out silicon dioxide and 100-700 parts of aluminum isopropoxide according to the silicon-to-aluminum ratio Si:Al = 180-220:1. Stir the mixture in the presence of a solvent until the aluminum isopropoxide is fully dissolved. Then add silicon dioxide and transfer the mixture to a reaction vessel. Aging is carried out at room temperature for 24 hours. The reaction vessel is then transferred to a 90°C oven and reacted for 4 hours. After centrifugation, washing, drying, and calcination, dry ZSM-5 filler is obtained.
[0014] (3) Synthesis of ZSM-5 filler and preparation of casting solution:
[0015] Weigh 500-800 parts of Pebax-1657 solution from (1) into a reagent bottle, and add 100-500 parts of the filler solution obtained in (2) above. Use a turbine oscillator to oscillate for 18-36s and sonicate for 15-30min. Then stir for 40-60min. After the filler and polymer solution are mixed evenly, let the casting solution stand to degas.
[0016] (4) Casting solution treatment and preparation of mixed matrix membranes:
[0017] The casting solution was subjected to ultrasonic degassing, and after standing, it was poured onto a polytetrafluoroethylene plate and dried in a constant temperature oven at 60-80℃ for 18-24 hours. Then, it was placed in a vacuum oven and vacuumed to continue desolvating for 18-24 hours to obtain a ZSM-5 mixed matrix membrane. After modification, a sulfur / molybdenum modified ZSM-5 mixed matrix membrane was obtained.
[0018] Based on the above technical solution, preferably, the solvent is one of tetrapropylammonium hydroxide, tetrapropylbromine hydroxide, ethanol, N,N-dimethylformamide, and N,N-diethylformamide.
[0019] Based on the above technical solution, preferably, the centrifuge speed is 7000-10000 and the centrifugation time is 5-10 min.
[0020] Based on the above technical solution, preferably, the mass ratio of ethanol to water is 6-9:1-4.
[0021] Based on the above technical solution, preferably, the solid content of the Pebax-1657 solution is 1-5%.
[0022] Based on the above technical solution, preferably, the mass fraction of pure ZSM-5 nanoparticles in the casting solution is 1-20 wt.%.
[0023] Based on the above technical solution, preferably, the ultrasonic method involves ultrasonic dispersion for 15–45 min, followed by stirring at 500–1000 rpm for 30–60 min at room temperature.
[0024] Based on the above technical solution, preferably, the drying time in the oven and the vacuum drying time are both 18 to 24 hours.
[0025] Based on the above technical solution, preferably, the modification method is as follows:
[0026] Immerse 100-150 parts of the cleaned ZSM-5 mixed matrix membrane in 1000-1500 parts of toluene, then add 3-7 parts of molybdenum dithiocarbamate, 0.3-3 parts of 1-(3-methylbut-2-en-1-yl)guanidine hydrochloride, and 2-5 parts of diethanolamine. Immerse at a temperature of 60-80℃ for 10-16 hours, then remove the ZSM-5 mixed matrix membrane and dry it.
[0027] The dried ZSM-5 mixed matrix membrane was placed in a plasma device and subjected to plasma treatment under the conditions of RF power of 50W to 150W, sulfur hexafluoride flow rate of 10 mL / min to 30 mL / min, and treatment time of 10 min to 30 min to obtain sulfur / molybdenum modified ZSM-5 mixed matrix membrane.
[0028] The modification mechanism involves the following: during plasma treatment, the active sulfur species generated from the decomposition of sulfur hexafluoride react chemically with the molybdenum / guanidine functional groups on the membrane surface to form stable sulfur / molybdenum compounds. These compounds provide additional active sites, enhancing the membrane material's adsorption and selective permeation capabilities for CO2.
[0029] Based on the above technical solution, the hybrid matrix membrane prepared by the present invention is used for CO2 / N2 gas separation.
[0030] The structural formulas of the substances mentioned above are as follows:
[0031] The structural formula of ZSM-5 is:
[0032]
[0033] The structural formula for pebax-1657 is:
[0034]
[0035] The basic principle of this invention:
[0036] Three-dimensional materials can create more gas molecule transport channels, significantly improving gas permeability. ZSM-5 is a dual-channel three-dimensional material with an appropriate pore size in the CO2 / N2 separation system, thereby creating a large number of directional transport channels for CO2 permeation within the membrane. At the same time, it utilizes its own silanol groups to generate a strong adsorption effect on CO2, effectively improving the selectivity of CO2 / N2, and ultimately achieving the goal of improving the CO2 separation performance of the mixed matrix membrane.
[0037] The beneficial effects achieved by the present invention using the above technical solution are as follows:
[0038] This invention prepares a hybrid matrix membrane by blending pebax-1657 as the matrix material and ZSM-5 as the filler.
[0039] 1. Superior mechanical properties:
[0040] Pebax is a block copolymer formed by blending polyether segments (PE) and amide segments (PA). The polyether segments exhibit rubber-like properties, ensuring that the membrane material itself has a high free volume fraction, which can provide good gas transport channels and reduce mass transfer resistance. At the same time, the large number of basic amine groups in the amide at the front end of the polyether have a strong interaction ability with CO2, which can improve the solubility of CO2 in the membrane, thereby effectively improving the membrane material's solubility selectivity for CO2 gas.
[0041] 2. Optimized design of porous ZSM-5 packing:
[0042] The introduction of ZSM-5 packing material, synthesized using TPAOH template agent, results in a highly compact fit between the organic molecules and the inorganic framework. Simultaneously, the organic structure-directing agent exhibits only one orientation within the pores or cages, preventing free movement and creating a porous packing material with a suitable pore size structure. This provides transport channels for CO2 within the membrane, facilitating efficient CO2 permeation.
[0043] 3. Enhancement effect of sulfur / molybdenum modification
[0044] Through dual modification using molybdenum ions and plasma treatment, the resistance during CO2 transport is reduced while maintaining the original mechanical strength, effectively improving the CO2 selectivity and permeability of the ZSM-5 mixed matrix membrane.
[0045] 4. The enhancing effect of hydroxyl groups:
[0046] The hydroxyl groups in the packing material further improve the adsorption performance of the membrane material for carbon dioxide, thus enhancing the membrane's separation effect.
[0047] 5. Environmentally friendly preparation process:
[0048] Using deionized water as a solvent aligns with environmental protection principles. The entire preparation process is mild and simple, with relatively low costs, providing a feasible method for green development.
[0049] 6. CO2 permeability and selectivity:
[0050] The hybrid matrix membrane exhibits good CO2 permeability (PCO2), reaching 72.62-95.26 Barrer, while the CO2 / N2 selectivity reaches 58.37-82.08. Attached Figure Description
[0051] Figure 1 This is the X-ray diffraction pattern of the synthesized material.
[0052] Figure 2The X-ray diffraction patterns are those of the hybrid matrix films obtained in Examples 1-3. The peak heights, from lowest to highest, correspond to the hybrid matrix films of Examples 1, 2, and 3, respectively.
[0053] Figure 3 The graph shows the performance of the hybrid matrix membranes obtained in Examples 1-3. Detailed Implementation
[0054] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with embodiments. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0055] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0056] Comparative Example
[0057] A method for improving the CO2 separation performance of a mixed matrix membrane using a topological molecular sieve (ZSM-5) is characterized by comprising the following steps:
[0058] (1) Preparation of Pebax-1657 solution:
[0059] 93g of Pebax-1657 and 3200g of ethanol / water were placed in a flask and magnetically stirred for 2.5h while maintaining a certain temperature to obtain a Pebax solution of uniform concentration.
[0060] (2) Casting solution treatment and matrix membrane preparation:
[0061] The casting solution was subjected to ultrasonic degassing, and after standing, it was poured onto a polytetrafluoroethylene plate and dried in an 80°C constant temperature oven for 18 hours. Then, it was placed in a vacuum oven for vacuum removal for another 18 hours to obtain the matrix membrane.
[0062] The mass ratio of ethanol to water is 6:1.
[0063] The Pebax-1657 solution has a solid content of 1%.
[0064] The ultrasonic method involves ultrasonic dispersion for 15 minutes, followed by stirring at 500 rpm for 30 minutes at room temperature.
[0065] The drying time in the oven and the vacuum drying time are both 18 hours.
[0066] Example 1
[0067] A method for improving the CO2 separation performance of a mixed matrix membrane using a topological molecular sieve (ZSM-5) is characterized by comprising the following steps:
[0068] (1) Preparation of Pebax-1657 solution:
[0069] 93g of Pebax-1657 and 3200g of ethanol / water were placed in a flask and magnetically stirred for 2.5h while maintaining a certain temperature to obtain a Pebax solution of uniform concentration.
[0070] (2) Preparation method of pure ZSM-5 filler:
[0071] Weigh out silicon dioxide and 100g of aluminum isopropoxide according to the silicon-to-aluminum ratio Si:Al = 180:1. Stir the mixture in the presence of solvent until the aluminum isopropoxide is fully dissolved. Then add silicon dioxide and transfer it to a reaction vessel. Let it age at room temperature for 24 hours. Then transfer the reaction vessel to a 90℃ oven and react for 4 hours. Centrifuge, wash, dry, and calcine to obtain dry ZSM-5 filler.
[0072] (3) Synthesis of ZSM-5 filler and preparation of casting solution:
[0073] Weigh 500g of Pebax-1657 solution from (1) into a reagent bottle, and add 100g of the filler solution obtained in (2) above. Use a turbine oscillator to oscillate for 18s and sonicate for 15min. Then stir for 40min. After the filler and polymer solution are mixed evenly, let the casting solution stand to degas.
[0074] (4) Casting solution treatment and preparation of mixed matrix membranes:
[0075] The casting solution was subjected to ultrasonic degassing, and after standing, it was poured onto a polytetrafluoroethylene plate and dried in an 80℃ constant temperature oven for 18 hours. Then, it was placed in a vacuum oven for vacuum removal for another 18 hours to obtain a ZSM-5 mixed matrix membrane. After modification, a sulfur / molybdenum modified ZSM-5 mixed matrix membrane was obtained.
[0076] The solvent is tetrapropylammonium hydroxide.
[0077] The centrifuge operates at a speed of 7000 rpm and a centrifugation time of 5 minutes.
[0078] The mass ratio of ethanol to water is 6:1.
[0079] The Pebax-1657 solution has a solid content of 1%.
[0080] The casting solution contains 10 wt.% pure ZSM-5 nanoparticles.
[0081] The ultrasonic method involves ultrasonic dispersion for 15 minutes, followed by stirring at 500 rpm for 30 minutes at room temperature.
[0082] The drying time in the oven and the vacuum drying time are both 18 hours.
[0083] The modification method is as follows:
[0084] Immerse 100g of cleaned ZSM-5 mixed matrix membrane in 1000g of toluene, then add 3g of molybdenum dithiocarbamate, 0.3g of 1-(3-methylbut-2-en-1-yl)guanidine hydrochloride, and 2g of diethanolamine. Immerse at 60℃ for 10h, then remove the ZSM-5 mixed matrix membrane and dry it.
[0085] The dried ZSM-5 mixed matrix membrane was placed in a plasma device and subjected to plasma treatment at a radio frequency power of 50W to 150W, a sulfur hexafluoride flow rate of 10 mL / min, and a treatment time of 30 minutes to obtain a sulfur / molybdenum modified ZSM-5 mixed matrix membrane.
[0086] Example 2
[0087] A method for improving the CO2 separation performance of a mixed matrix membrane using a topological molecular sieve (ZSM-5) is characterized by comprising the following steps:
[0088] (1) Preparation of Pebax-1657 solution:
[0089] 117g of Pebax-1657 and 4700g of ethanol / water were placed in a flask and magnetically stirred for 3.5h while maintaining a certain temperature to obtain a Pebax solution of uniform concentration.
[0090] (2) Preparation method of pure ZSM-5 filler:
[0091] Weigh out silicon dioxide and 350g of aluminum isopropoxide according to the silicon-to-aluminum ratio Si:Al = 200:1. Stir the mixture in the presence of solvent until the aluminum isopropoxide is fully dissolved. Then add silicon dioxide and transfer the mixture to a reaction vessel. Let it age at room temperature for 24 hours. Then transfer the reaction vessel to a 90℃ oven and react for 4 hours. Centrifuge, wash, dry, and calcine to obtain dry ZSM-5 filler.
[0092] (3) Synthesis of ZSM-5 filler and preparation of casting solution:
[0093] Weigh 650g of Pebax-1657 solution from (1) into a reagent bottle, and add 300g of the filler solution obtained in (2) above. Use a turbine oscillator to oscillate for 24s and sonicate for 24min. Then stir for 50min. After the filler and polymer solution are mixed evenly, let the casting solution stand to degas.
[0094] (4) Casting solution treatment and preparation of mixed matrix membranes:
[0095] The casting solution was subjected to ultrasonic degassing, and after standing, it was poured onto a polytetrafluoroethylene plate and dried in a 70°C constant temperature oven for 21 hours. Then, it was placed in a vacuum oven for vacuum removal for another 21 hours to obtain a ZSM-5 mixed matrix membrane. After modification, a sulfur / molybdenum modified ZSM-5 mixed matrix membrane was obtained.
[0096] The solvent is tetrapropyl bromide hydroxide.
[0097] The centrifuge operates at a speed of 8500 rpm and a centrifugation time of 7.5 minutes.
[0098] The mass ratio of ethanol to water is 9:2.
[0099] The Pebax-1657 solution has a solid content of 3%.
[0100] The casting solution contains 15 wt.% pure ZSM-5 nanoparticles.
[0101] The ultrasonic method involves ultrasonic dispersion for 30 minutes, followed by stirring at 750 rpm for 45 minutes at room temperature.
[0102] The drying time in the oven and the vacuum drying time are both 21 hours.
[0103] The modification method is as follows:
[0104] Immerse 125g of the cleaned ZSM-5 mixed matrix membrane in 1250g of toluene, then add 5g of molybdenum dithiocarbamate, 1.8g of 1-(3-methylbut-2-en-1-yl)guanidine hydrochloride, and 3.5g of diethanolamine. Immerse at 70℃ for 13.5h, then remove the ZSM-5 mixed matrix membrane and dry it.
[0105] The dried ZSM-5 mixed matrix membrane was placed in a plasma device and subjected to plasma treatment at a radio frequency power of 50W to 150W, a sulfur hexafluoride flow rate of 20 mL / min, and a treatment time of 20 minutes to obtain a sulfur / molybdenum modified ZSM-5 mixed matrix membrane.
[0106] Example 3
[0107] A method for improving the CO2 separation performance of a mixed matrix membrane using a topological molecular sieve (ZSM-5) is characterized by comprising the following steps:
[0108] (1) Preparation of Pebax-1657 solution:
[0109] 137g of Pebax-1657 and 4200g of ethanol / water were placed in a flask and magnetically stirred for 5 hours while maintaining a certain temperature to obtain a Pebax solution of uniform concentration.
[0110] (2) Preparation method of pure ZSM-5 filler:
[0111] Weigh out silicon dioxide and 700g of aluminum isopropoxide according to the silicon-to-aluminum ratio Si:Al = 220:1. Stir the mixture in the presence of solvent until the aluminum isopropoxide is fully dissolved. Then add silicon dioxide and transfer the mixture to a reaction vessel. Let it age at room temperature for 24 hours. Then transfer the reaction vessel to a 90℃ oven and react for 4 hours. Centrifuge, wash, dry, and calcine to obtain dry ZSM-5 filler.
[0112] (3) Synthesis of ZSM-5 filler and preparation of casting solution:
[0113] Weigh 800g of Pebax-1657 solution from (1) into a reagent bottle, and add 500g of the filler solution obtained in (2) above. Use a turbine oscillator to oscillate for 36s and sonicate for 30min. Then stir for 60min. After the filler and polymer solution are mixed evenly, let the casting solution stand to degas.
[0114] (4) Casting solution treatment and preparation of mixed matrix membranes:
[0115] The casting solution was subjected to ultrasonic degassing, and after standing, it was poured onto a polytetrafluoroethylene plate and dried in an 80°C constant temperature oven for 24 hours. Then, it was placed in a vacuum oven for vacuum removal for another 24 hours to obtain a ZSM-5 mixed matrix membrane. After modification, a sulfur / molybdenum modified ZSM-5 mixed matrix membrane was obtained.
[0116] The solvent is N,N-dimethylformamide.
[0117] The centrifuge operates at a speed of 10,000 rpm and a centrifugation time of 10 minutes.
[0118] The mass ratio of ethanol to water is 9:4.
[0119] The Pebax-1657 solution has a solid content of 5%.
[0120] The casting solution contains 20 wt.% pure ZSM-5 nanoparticles.
[0121] The ultrasonic method involves ultrasonic dispersion for 45 minutes, followed by stirring at 1000 rpm for 60 minutes at room temperature.
[0122] The drying time in the oven and the vacuum drying time are both 24 hours.
[0123] The modification method is as follows:
[0124] Immerse 150g of the cleaned ZSM-5 mixed matrix membrane in 1500g of toluene, then add 7g of molybdenum dithiocarbamate, 3g of 1-(3-methylbut-2-en-1-yl)guanidine hydrochloride and 5g of diethanolamine. Immerse at 80℃ for 16h, then remove the ZSM-5 mixed matrix membrane and dry it.
[0125] The dried ZSM-5 mixed matrix membrane was placed in a plasma device and subjected to plasma treatment at a radio frequency power of 50W to 150W, a sulfur hexafluoride flow rate of 30 mL / min, and a treatment time of 10 minutes to obtain a sulfur / molybdenum modified ZSM-5 mixed matrix membrane.
[0126] Table 1 shows the component ratios and related performance test results of the comparative examples, Examples 1-3, and the prepared mixed matrix membranes:
[0127] Table 1
[0128]
[0129] As can be seen from Table 1, the post-mixed matrix membranes described in Examples 1 to 3 of the present invention have better permeability and excellent selectivity compared to pure membranes.
[0130] The present invention has been described above through specific embodiments and examples. However, these descriptions are merely illustrative and should not be construed as limiting the scope of protection of the present invention. Without departing from the spirit and scope of the present invention, those skilled in the art can make various improvements, modifications, or equivalent substitutions to the technical solutions and implementation methods of the present invention, and all such modifications and substitutions should fall within the scope of protection of the present invention.
Claims
1. A method for preparing a ZSM-5 mixed matrix membrane for CO2 separation, characterized in that, The method includes the following steps: (1) Preparation of Pebax-1657 solution: 93-137 parts of Pebax-1657 and 3200-4200 parts of ethanol aqueous solution were placed in a flask and magnetically stirred for 2.5-5 hours while maintaining a certain temperature to obtain a Pebax solution of uniform concentration. (2) Preparation method of ZSM-5 packing: Weigh out silicon dioxide and 100-700 parts of aluminum isopropoxide according to the silicon-to-aluminum ratio Si:Al=180-220:
1. Stir the mixture in the presence of solvent until the aluminum isopropoxide is fully dissolved. Then add silicon dioxide and transfer it to a reaction vessel. Aging at room temperature for 24 hours, then transfer the reaction vessel to a 90℃ oven for 4 hours. Centrifuge, wash, dry, and calcine to obtain dry ZSM-5 filler. (3) Preparation of casting solution: Weigh 500-800 parts of Pebax-1657 solution from (1) into a reagent bottle, and add 100-500 parts of the filler solution obtained in (2) above. Use a turbine oscillator to oscillate for 18-36s and sonicate for 15-30min. Then stir for 40-60min. After the filler and polymer solution are mixed evenly, let the casting solution stand to degas. (4) Preparation of hybrid matrix membranes: After stirring the casting solution, ultrasonic degassing was performed. After standing, the solution was poured onto a polytetrafluoroethylene plate and dried in a constant temperature oven at 60-80℃ for 18-24 hours. Then, it was placed in a vacuum oven and vacuumed to continue desolventizing for 18-24 hours to obtain a ZSM-5 mixed matrix membrane. After modification, a sulfur / molybdenum modified ZSM-5 mixed matrix membrane was obtained. The modification method is as follows: Immerse 100-150 parts of the cleaned ZSM-5 mixed matrix membrane in 1000-1500 parts of toluene, then add 3-7 parts of molybdenum dithiocarbamate, 0.3-3 parts of 1-(3-methylbut-2-en-1-yl)guanidine hydrochloride, and 2-5 parts of diethanolamine. Immerse at a temperature of 60-80℃ for 10-16 hours, then remove the ZSM-5 mixed matrix membrane and dry it. The dried ZSM-5 mixed matrix membrane was placed in a plasma device and subjected to plasma treatment under the conditions of RF power of 50W to 150W, sulfur hexafluoride flow rate of 10 mL / min to 30 mL / min, and treatment time of 10 min to 30 min to obtain sulfur / molybdenum modified ZSM-5 mixed matrix membrane.
2. The method for preparing a ZSM-5 mixed matrix membrane for CO2 separation according to claim 1, characterized in that, The solvent is one of tetrapropylammonium hydroxide, tetrapropylbromine hydroxide, ethanol, N,N-dimethylformamide, and N,N-diethylformamide.
3. The method for preparing a ZSM-5 mixed matrix membrane for CO2 separation according to claim 1, characterized in that, The centrifugation speed is 7000-10000, and the centrifugation time is 5-10 minutes.
4. The method for preparing a ZSM-5 mixed matrix membrane for CO2 separation according to claim 1, characterized in that, The mass ratio of ethanol to water in the ethanol-water solution is 6-9:1-4.
5. The method for preparing a ZSM-5 mixed matrix membrane for CO2 separation according to claim 1, characterized in that, The Pebax-1657 solution has a solid content of 1-5%.
6. The method for preparing a ZSM-5 mixed matrix membrane for CO2 separation according to claim 1, characterized in that, The mass fraction of pure ZSM-5 nanoparticles in the casting solution is 1–20 wt.
7. The method for preparing a ZSM-5 mixed matrix membrane for CO2 separation according to claim 1, characterized in that, The ultrasonic method involves stirring at 500–1000 rpm for 30–60 min at room temperature, followed by ultrasonic dispersion for 15–45 min.
8. The method for preparing a ZSM-5 mixed matrix membrane for CO2 separation according to claim 1, characterized in that, The drying time in the oven and the vacuum drying time are both 18 to 24 hours.
9. The mixed matrix membrane prepared by the preparation method according to any one of claims 1-8, characterized in that, This hybrid matrix membrane is used for CO2 / N2 gas separation.
Citation Information
Patent Citations
Preparation method and application of mixed matrix membrane with thermoplastic elastomer as matrix
CN104689730A
Carbon dioxide separation and recovery system in exhaust gas by zeolite membrane
JP2012236123A