One-dimensional Zn / Cu monatomic alloy catalyst, preparation method and application thereof

By constructing a Zn-based MOF layer on the surface of Cu nanowires and calcining it at high temperature to form a one-dimensional Zn/Cu single-atom alloy catalyst, the problems of low efficiency and poor stability of existing catalysts in the process of CO₂ hydrogenation to methanol were solved, and a high-efficiency and stable catalytic effect was achieved.

CN118105982BActive Publication Date: 2026-11-24NANKAI UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410117177.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-29
Publication Date
2026-11-24
Estimated Expiration
2044-01-29

AI Technical Summary

Technical Problem

Existing catalysts are prone to side reactions during the hydrogenation of CO₂ to methanol, resulting in low conversion efficiency and poor stability, which cannot meet the requirements for high-efficiency catalysis.

Method used

By constructing a Zn-based MOF layer on the surface of Cu nanowires and calcining it at high temperature under an inert atmosphere to form a one-dimensional Zn/Cu single-atom alloy catalyst, the sintering and agglomeration of Cu nanowires are avoided, thereby improving catalytic activity and stability.

Benefits of technology

The catalyst achieved high selectivity and efficiency in the preparation of methanol by CO₂ hydrogenation. The methanol selectivity was 100% in the range of 150–210 °C, and it also had excellent stability, avoiding the aggregation of Cu nanostructures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118105982B_ABST
    Figure CN118105982B_ABST
Patent Text Reader

Abstract

This invention provides a one-dimensional Zn / Cu single-atom alloy catalyst, its preparation method, and its application. The preparation steps include: 1) preparing one-dimensional Cu nanomaterials; 2) dispersing the obtained one-dimensional Cu nanomaterials in an organic solvent, sonicating and degassing, sequentially adding a degassed organic ligand solution and a Zn ion solution, and washing after settling and centrifugation to obtain Zn-based MOF-coated one-dimensional Cu nanomaterials; 3) calcining the obtained Zn-based MOF-coated one-dimensional Cu nanomaterials under an inert atmosphere and at high temperature to obtain the one-dimensional Zn / Cu single-atom alloy catalyst. The one-dimensional Zn / Cu single-atom alloy material obtained by this invention can be used as a catalyst for the thermocatalytic hydrogenation of CO2 to methanol in the energy field, providing a theoretical and practical basis for achieving the goal of zero carbon emissions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalyst material preparation technology, and relates to a method for preparing a one-dimensional Zn / Cu single-atom alloy catalyst. Background Technology

[0002] Research into new materials helps people understand the properties of matter, explore mechanisms in depth, and meet the demands of today's changing times. Meanwhile, global climate change has caused a severe crisis for the sustainable development of human society and the entire ecosystem. The massive emissions of greenhouse gases such as carbon dioxide (CO2) are one of the main causes of global climate change; therefore, controlling CO2 emissions is a crucial means of addressing global climate change. On the other hand, the vast reserves of CO2 in the atmosphere can also serve as a rich renewable carbon resource for the synthesis of fuels and chemicals. Among various CO2 conversion and utilization pathways, the hydrogenation of CO2 to synthesize green CH3OH is one of the best ways to achieve this goal.

[0003] However, the conversion of CO2 into methanol requires a large amount of energy, necessitating highly active catalysts. Current catalytic CO2 hydrogenation materials are prone to drawbacks during the reaction process, such as (1) initiating side reactions and low conversion efficiency; and (2) low stability. Therefore, it is urgent to supplement and develop catalysts using new materials. Summary of the Invention

[0004] The purpose of this invention is to address the aforementioned problems in the existing technology and to provide a method for preparing a Zn / Cu alloy, which introduces Zn into Cu through calcination, unlike electrochemical displacement. Furthermore, this material can be applied to the thermocatalytic hydrogenation of CO2 to produce methanol.

[0005] Technical solution of the present invention

[0006] A method for preparing a one-dimensional Zn / Cu single-atom alloy catalyst includes the following steps:

[0007] Step 1, Construction of one-dimensional Cu nanomaterials: The Cu precursor solution is heated and stirred (stirring temperature is 45-50℃), and then subjected to sonication, hydrothermal reaction, centrifugation and washing in sequence to obtain Cu nanowires;

[0008] Step 2, Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial: The one-dimensional Cu nanowires obtained in step 1 are dispersed in an organic solvent, sonicated and degassed, and the degassed organic ligand solution and (Zn(NO3)2) solution are added in sequence. After standing for 1-2 hours, the one-dimensional Cu nanomaterials are obtained by centrifugation and washing.

[0009] Step 3, Preparation of one-dimensional Zn / Cu single-atom alloy catalyst: The one-dimensional Cu nanomaterials wrapped with Zn-based MOF obtained in step 2 are calcined in an inert atmosphere at high temperature to obtain the one-dimensional Zn / Cu single-atom alloy catalyst.

[0010] As a preferred embodiment, the Cu precursor solution is an aqueous solution containing CuCl2·2H2O, HDA, and D-(+)-glucose. The molar ratio of CuCl2·2H2O, D-(+)-glucose, and HDA is 1:(1.21-1.27):(4.10-4.18).

[0011] As a preferred embodiment, the organic solvent is 0.028-0.032 mol / mL. -1 A methanol solution of CTAB.

[0012] As a preferred embodiment, the organic ligand solution is a methanol solution of 2-methylimidazole.

[0013] As a preferred option, the mass ratio of 2-methylimidazole to Zn(NO3)2 is 1 to 1.2.

[0014] As a preferred embodiment, the hydrothermal reaction conditions are 115-125℃ for 11.8-13 hours.

[0015] As a preferred embodiment, the inert atmosphere is argon, and the high-temperature calcination conditions are argon (flow rate 15-25 mL / min). –1 ) below 2-5℃ min –1 Heat to 800℃ for 2-3 hours at the specified heating rate.

[0016] This invention also provides a one-dimensional Zn / Cu single-atom alloy catalyst prepared by the above method, and its application in the thermocatalytic CO2 hydrogenation to methanol reaction.

[0017] Advantages and beneficial effects of the present invention:

[0018] This invention avoids sintering and agglomeration during the calcination of copper nanowires. The MOF layer on the surface of the one-dimensional Cu nanomaterial can effectively protect the copper nanowires and prevent oxidation. Attached Figure Description

[0019] Figure 1 A schematic diagram of the synthesis route for the one-dimensional Zn / Cu single-atom alloy catalyst provided by this invention.

[0020] Figure 2 The image shows the X-ray diffraction pattern of the one-dimensional Zn / Cu single-atom alloy catalyst obtained in Example 1.

[0021] Figure 3The image shows a TEM image of Zn / Cu SAAs obtained in Example 1.

[0022] Figure 4 The image shows the EELS plot of Zn / Cu SAAs obtained in Example 1.

[0023] Figure 5 The images show (a) the K-edge XANES spectrum of Zn in Zn / Cu SAAs, (b) the K-edge EXAFS oscillation function of Zn, (c) the K-edge XANES spectrum of Cu, and (d) the K-edge EXAFS oscillation function of Cu obtained in Example 1.

[0024] Figure 6 The inset shows the Cu 2p XPS spectra of (a) Cu NWS and Zn / Cu SAAS obtained in Example 1, with the Cu 2p spectrum shown in the inset. 3 / 2 (a) Enlarged view; (b) Zn 2p XPS spectrum of Zn / Cu SAAS.

[0025] Figure 7 The graph shows the relationship between the selectivity of CH3OH prepared by CO2 hydrogenation on Zn / Cu SAAs obtained in Example 1 and the reaction temperature.

[0026] Figure 8 The graph shows the relationship between the yield of CH3OH prepared by CO2 hydrogenation on Zn / Cu SAAs obtained in Example 1 and the reaction temperature. Detailed Implementation

[0027] Example 1: Preparation of one-dimensional Zn / Cu single-atom alloy catalyst, the synthetic route is as follows: Figure 1 As shown.

[0028] (1) Construction of one-dimensional Cu nanomaterials:

[0029] A 40 mL aqueous solution containing 85 mg CuCl₂·2H₂O, 500 mg HDA, and 111 mg D-(+)-glucose was vigorously stirred overnight at 45 °C to obtain a light blue emulsion mixture, which was then sonicated for 20 minutes. The solution was transferred to a 100 mL stainless steel autoclave lined with PTFE. After hydrothermal reaction at 120 °C for 12 hours, the solution was cooled to room temperature to obtain a brown mixture. The solid product obtained by centrifugation (10,000 rpm, 5 minutes) was washed three times with water, ethanol, and hexane, respectively, to obtain Cu nanowires. Finally, the Cu nanowires were stored in 8 mL of anhydrous ethanol.

[0030] (2) Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial

[0031] Two mL of freshly synthesized Cu nanowire ethanol dispersion was dispersed in 18 mL of degassed methanol solution containing 200 mg CTAB, and the solution was sonicated for 20 min followed by degassed for 10 min. Then, 54 mg of 2-methylimidazole and 50 mg of Zn(NO3)2·6H2O were dissolved in 5 mL of degassed methanol, respectively. Finally, under nitrogen protection, the methanol solution of 2-methylimidazole and Zn(NO3)2·6H2O were added sequentially to the one-dimensional Cu nanowires dispersed in the organic solvent. The vial was sealed with a diaphragm and left to stand at room temperature for 1 hour without stirring. The suspension was collected by centrifugation under air-free conditions and washed three times with degassed methanol. The solid product was obtained by centrifugation and then vacuum dried overnight at room temperature to obtain the Zn-based MOF-encapsulated one-dimensional Cu nanomaterial Cu NWs@ZIF-8.

[0032] (3) Preparation of one-dimensional Zn / Cu single-atom alloy catalysts

[0033] A one-dimensional Zn / Cu single-atom alloy catalyst was synthesized by direct carbonization of Cu NWs@ZIF-8 prepared in step (2) under an argon flow at 800 °C. The prepared Cu NWs@ZIF-8 was placed in a tube furnace and heated to 20 mL min. –1 At an argon flow rate of 3℃ / min –1 The sample was heated to 800°C for 2 hours at a heating rate of [missing information]. After calcination, the sample was cooled to room temperature to obtain a one-dimensional Zn / Cu single-atom alloy catalyst, CuZn / Cu SAAs.

[0034] (4) Characterization and testing

[0035] Characterization: The one-dimensional Zn / Cu single-atom alloy catalyst obtained in Example 1 was characterized in various ways, and the results are as follows: Figures 2-7 As shown.

[0036] Figure 2 The image shows the X-ray diffraction (XRD) pattern of the one-dimensional Zn / Cu single-atom alloy catalyst obtained in Example 1, which confirms the formation of the Zn / Cu single-atom alloy.

[0037] Figure 3 The image shows a TEM image of the Zn / Cu SAAs obtained in Example 1. The results indicate that the obtained alloy material is a nanowire with a width of about 20 nm.

[0038] Figure 4 The image shows the EELS plot of the Zn / Cu SAAs obtained in Example 1. The results indicate that Cu and Zn are uniformly distributed in the obtained alloy material.

[0039] Figure 5The images show (a) the K-edge XANES spectrum of Zn in the Zn / Cu SAAs obtained in Example 1, (b) the K-edge EXAFS oscillation function of Zn, (c) the K-edge XANES spectrum of Cu, and (d) the K-edge EXAFS oscillation function of Cu. The results indicate that only Cu-Cu and a small amount of Zn-Cu exist in the alloy material.

[0040] Figure 6 The inset shows the Cu 2p XPS spectra of (a) Cu NWS and Zn / Cu SAAS obtained in Example 1, with the Cu 2p spectrum shown in the inset. 3 / 2 (a) Enlarged view; (b) Zn 2p XPS spectrum of Zn / Cu SAAS. The results show that electrons are transferred from Zn to the adjacent Cu, confirming the single-atom dispersion of Zn atoms in Zn / Cu SAAS.

[0041] Catalytic hydrogenation of carbon dioxide

[0042] The catalytic activity of the prepared catalyst for CO2 hydrogenation was evaluated using a high-pressure reactor at 3 MPa (H2 / CO2 = 3 / 1) and 100 °C. 20 mg of catalyst was placed in a 50 mL high-pressure, PTFE-lined stainless steel reactor. The CO2 hydrogenation reaction was carried out for 12 h at different temperatures (150–250 °C, 3 MPa, H2 / CO2 = 3). After the reaction, when the temperature cooled to room temperature, 5 mL of anhydrous THF was added to the reactor to extract the liquid product. The gaseous product was quantitatively analyzed by gas chromatography equipped with a thermal conductivity detector and a flame ionization detector. The liquid product was analyzed by NMR and GC.

[0043] Within the temperature range of 150–210 °C, the Zn / Cu SAAs prepared by this invention exhibited 100% selectivity for methanol, and the methanol yield increased with increasing temperature. At 190 °C, the highest methanol yield reached 853.9 μmol g. -1 h -1 When the reaction temperature exceeds 210℃, the byproduct CO appears and gradually increases until the reaction temperature exceeds 250℃, at which point the product CH3OH is completely converted to CO. In addition, the Zn / Cu SAAs catalyst synthesized in this study exhibits excellent stability, with no aggregation of Cu nanostructures after the reaction. The results of thermocatalytic CO2 hydrogenation are as follows: Figure 7 As shown in Figure 8.

[0044] Example 2: Preparation of one-dimensional Zn / Cu single-atom alloy catalyst

[0045] (1) Construction of one-dimensional Cu nanomaterials:

[0046] A 40 mL aqueous solution containing 85 mg CuCl₂·2H₂O, 500 mg HDA, and 111 mg D-(+)-glucose was vigorously stirred overnight at 45 °C to obtain a light blue emulsion mixture, which was then sonicated for 20 minutes. The solution was transferred to a 100 mL stainless steel autoclave lined with PTFE. After hydrothermal reaction at 120 °C for 12 hours, the solution was cooled to room temperature to obtain a brown mixture. The solid product obtained by centrifugation (10,000 rpm, 5 min) was washed three times with water, ethanol, and hexane, respectively. Finally, the Cu nanowires were stored in 8 mL of anhydrous ethanol.

[0047] (2) Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial

[0048] Two mL of freshly synthesized Cu nanowire ethanol dispersion was dispersed in 18 mL of degassed methanol solution containing 200 mg CTAB, and the solution was sonicated for 20 min followed by degassed for 10 min. Then, 67.5 mg 2-methylimidazole and 62.5 mg Zn(NO3)2·6H2O were dissolved in 5 mL of degassed methanol, respectively. Finally, under nitrogen protection, the methanol solution of 2-methylimidazole and Zn(NO3)2·6H2O were added sequentially to the one-dimensional Cu nanowires dispersed in the organic solvent. The vial was sealed with a diaphragm and left to stand at room temperature for 1 hour without stirring. The suspension was collected by centrifugation under air-free conditions and washed three times with degassed methanol. The solid product was obtained by centrifugation and then vacuum dried overnight at room temperature to obtain the Zn-based MOF-encapsulated one-dimensional Cu nanomaterial Cu NWs@ZIF-8.

[0049] (3) Preparation of one-dimensional Zn / Cu single-atom alloy catalysts

[0050] A one-dimensional Zn / Cu single-atom alloy catalyst was synthesized by direct carbonization of Cu NWs@ZIF-8 prepared in step (2) under an argon flow at 800 °C. The prepared Cu NWs@ZIF-8 was placed in a tube furnace and heated to 20 mL min. –1 At an argon flow rate of 3℃ / min –1 The sample was heated to 800°C for 2 hours at a heating rate of [missing information]. After calcination, the sample was cooled to room temperature to obtain a one-dimensional Zn / Cu single-atom alloy catalyst, CuZn / Cu SAAs.

[0051] Example 3: Preparation of one-dimensional Zn / Cu single-atom alloy catalyst

[0052] (1) Construction of one-dimensional Cu nanomaterials:

[0053] A 40 mL aqueous solution containing 85 mg CuCl₂·2H₂O, 500 mg HDA, and 111 mg D-(+)-glucose was vigorously stirred overnight at 45 °C to obtain a light blue emulsion mixture, which was then sonicated for 20 minutes. The solution was transferred to a 100 mL stainless steel autoclave lined with PTFE. After hydrothermal reaction at 120 °C for 12 hours, the solution was cooled to room temperature to obtain a brown mixture. The solid product obtained by centrifugation (10,000 rpm, 5 min) was washed three times with water, ethanol, and hexane, respectively. Finally, the Cu nanowires were stored in 8 mL of anhydrous ethanol.

[0054] (2) Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial

[0055] Two mL of freshly synthesized Cu nanowire ethanol dispersion was dispersed in 18 mL of degassed methanol solution containing 200 mg CTAB, and the solution was sonicated for 20 min followed by degassed for 10 min. Then, 40.5 mg 2-methylimidazole and 37.5 mg Zn(NO3)2·6H2O were dissolved in 5 mL of degassed methanol, respectively. Finally, under nitrogen protection, the methanol solution of 2-methylimidazole and Zn(NO3)2·6H2O were added sequentially to the one-dimensional Cu nanowires dispersed in the organic solvent. The vial was sealed with a diaphragm and left to stand at room temperature for 1 hour without stirring. The suspension was collected by centrifugation under air-free conditions and washed three times with degassed methanol. The solid product was obtained by centrifugation and then vacuum dried overnight at room temperature to obtain the Zn-based MOF-encapsulated one-dimensional Cu nanomaterial Cu NWs@ZIF-8.

[0056] (3) Preparation of one-dimensional Zn / Cu single-atom alloy catalysts

[0057] A one-dimensional Zn / Cu single-atom alloy catalyst was synthesized by direct carbonization of Cu NWs@ZIF-8 prepared in step (2) under an argon flow at 800 °C. The prepared Cu NWs@ZIF-8 was placed in a tube furnace and heated to 20 mL min. –1 At an argon flow rate of 3℃ / min –1 The sample was heated to 800°C for 2 hours at a heating rate of [missing information]. After calcination, the sample was cooled to room temperature to obtain a one-dimensional Zn / Cu single-atom alloy catalyst, CuZn / Cu SAAs.

[0058] Example 4: Preparation of one-dimensional Zn / Cu single-atom alloy catalyst

[0059] (1) Construction of one-dimensional Cu nanomaterials:

[0060] A 40 mL aqueous solution containing 85 mg CuCl₂·2H₂O, 500 mg HDA, and 111 mg D-(+)-glucose was vigorously stirred overnight at 50 °C to obtain a light blue emulsion mixture, which was then sonicated for 20 minutes. The solution was transferred to a 100 mL stainless steel autoclave lined with PTFE. After hydrothermal reaction at 120 °C for 12 hours, the solution was cooled to room temperature to obtain a brown mixture. The solid product obtained by centrifugation (10,000 rpm, 5 minutes) was washed three times with water, ethanol, and hexane, respectively, to obtain Cu nanowires. Finally, the Cu nanowires were stored in 8 mL of anhydrous ethanol.

[0061] (2) Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial

[0062] Two mL of freshly synthesized Cu nanowire ethanol dispersion was dispersed in 18 mL of degassed methanol solution containing 200 mg CTAB, and the solution was sonicated for 20 min followed by degassed for 10 min. Then, 54 mg of 2-methylimidazole and 50 mg of Zn(NO3)2·6H2O were dissolved in 5 mL of degassed methanol, respectively. Finally, under nitrogen protection, the methanol solution of 2-methylimidazole and Zn(NO3)2·6H2O were added sequentially to the one-dimensional Cu nanowires dispersed in the organic solvent. The vial was sealed with a diaphragm and left to stand at room temperature for 1 hour without stirring. The suspension was collected by centrifugation under air-free conditions and washed three times with degassed methanol. The solid product was obtained by centrifugation and then vacuum dried overnight at room temperature to obtain the Zn-based MOF-encapsulated one-dimensional Cu nanomaterial Cu NWs@ZIF-8.

[0063] (3) Preparation of one-dimensional Zn / Cu single-atom alloy catalysts

[0064] A one-dimensional Zn / Cu single-atom alloy catalyst was synthesized by direct carbonization of Cu NWs@ZIF-8 prepared in step (2) under an argon flow at 800 °C. The prepared Cu NWs@ZIF-8 was placed in a tube furnace and heated to 20 mL min. –1 At an argon flow rate of 3℃ / min –1 The sample was heated to 800°C for 2 hours at a heating rate of [missing information]. After calcination, the sample was cooled to room temperature to obtain a one-dimensional Zn / Cu single-atom alloy catalyst, CuZn / Cu SAAs.

[0065] Example 5: Preparation of one-dimensional Zn / Cu single-atom alloy catalyst

[0066] (1) Construction of one-dimensional Cu nanomaterials:

[0067] A 40 mL aqueous solution containing 85 mg CuCl₂·2H₂O, 500 mg HDA, and 111 mg D-(+)-glucose was vigorously stirred overnight at 45 °C to obtain a light blue emulsion mixture, which was then sonicated for 20 minutes. The solution was transferred to a 100 mL stainless steel autoclave lined with PTFE. After hydrothermal reaction at 120 °C for 12 hours, the solution was cooled to room temperature to obtain a brown mixture. The solid product obtained by centrifugation (10,000 rpm, 5 minutes) was washed three times with water, ethanol, and hexane, respectively, to obtain Cu nanowires. Finally, the Cu nanowires were stored in 8 mL of anhydrous ethanol.

[0068] (2) Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial

[0069] Two mL of freshly synthesized Cu nanowire ethanol dispersion was dispersed in 18 mL of degassed methanol solution containing 200 mg CTAB, and the solution was sonicated for 20 min followed by degassed for 10 min. Then, 54 mg of 2-methylimidazole and 50 mg of Zn(NO3)2·6H2O were dissolved in 5 mL of degassed methanol, respectively. Finally, under nitrogen protection, the methanol solution of 2-methylimidazole and Zn(NO3)2·6H2O were added sequentially to the one-dimensional Cu nanowires dispersed in the organic solvent. The vial was sealed with a diaphragm and left to stand at room temperature for 2 hours without stirring. The suspension was collected by centrifugation under air-free conditions and washed three times with degassed methanol. The solid product was obtained by centrifugation and then vacuum dried overnight at room temperature to obtain the Zn-based MOF-encapsulated one-dimensional Cu nanomaterial Cu NWs@ZIF-8.

[0070] (3) Preparation of one-dimensional Zn / Cu single-atom alloy catalysts

[0071] A one-dimensional Zn / Cu single-atom alloy catalyst was synthesized by direct carbonization of Cu NWs@ZIF-8 prepared in step (2) under an argon flow at 800 °C. The prepared Cu NWs@ZIF-8 was placed in a tube furnace and heated to 20 mL min. –1 At an argon flow rate of 3℃ / min –1 The sample was heated to 800°C for 2 hours at a heating rate of [missing information]. After calcination, the sample was cooled to room temperature to obtain a one-dimensional Zn / Cu single-atom alloy catalyst, CuZn / Cu SAAs.

[0072] Example 6: Preparation of one-dimensional Zn / Cu single-atom alloy catalyst

[0073] (1) Construction of one-dimensional Cu nanomaterials:

[0074] A 40 mL aqueous solution containing 85 mg CuCl₂·2H₂O, 500 mg HDA, and 111 mg D-(+)-glucose was vigorously stirred overnight at 45 °C to obtain a light blue emulsion mixture, which was then sonicated for 20 minutes. The solution was transferred to a 100 mL stainless steel autoclave lined with PTFE. After hydrothermal reaction at 120 °C for 12 hours, the solution was cooled to room temperature to obtain a brown mixture. The solid product obtained by centrifugation (10,000 rpm, 5 minutes) was washed three times with water, ethanol, and hexane, respectively, to obtain Cu nanowires. Finally, the Cu nanowires were stored in 8 mL of anhydrous ethanol.

[0075] (2) Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial

[0076] Two mL of freshly synthesized Cu nanowire ethanol dispersion was dispersed in 18 mL of degassed methanol solution containing 200 mg CTAB, and the solution was sonicated for 20 min followed by degassed for 10 min. Then, 54 mg of 2-methylimidazole and 50 mg of Zn(NO3)2·6H2O were dissolved in 5 mL of degassed methanol, respectively. Finally, under nitrogen protection, the methanol solution of 2-methylimidazole and Zn(NO3)2·6H2O were added sequentially to the one-dimensional Cu nanowires dispersed in the organic solvent. The vial was sealed with a diaphragm and left to stand at room temperature for 1 hour without stirring. The suspension was collected by centrifugation under air-free conditions and washed three times with degassed methanol. The solid product was obtained by centrifugation and then vacuum dried overnight at room temperature to obtain the Zn-based MOF-encapsulated one-dimensional Cu nanomaterial Cu NWs@ZIF-8.

[0077] (3) Preparation of one-dimensional Zn / Cu single-atom alloy catalysts

[0078] A one-dimensional Zn / Cu single-atom alloy catalyst was synthesized by direct carbonization of Cu NWs@ZIF-8 prepared in step (2) under an argon flow at 800 °C. The prepared Cu NWs@ZIF-8 was placed in a tube furnace and heated to 25 mL / min. –1 At an argon flow rate of 3℃ / min –1 The sample was heated to 800°C for 2 hours at a heating rate of [missing information]. After calcination, the sample was cooled to room temperature to obtain a one-dimensional Zn / Cu single-atom alloy catalyst, CuZn / Cu SAAs.

[0079] Example 7: Preparation of one-dimensional Zn / Cu single-atom alloy catalyst

[0080] (1) Construction of one-dimensional Cu nanomaterials:

[0081] A 40 mL aqueous solution containing 85 mg CuCl₂·2H₂O, 500 mg HDA, and 111 mg D-(+)-glucose was vigorously stirred overnight at 45 °C to obtain a light blue emulsion mixture, which was then sonicated for 20 minutes. The solution was transferred to a 100 mL stainless steel autoclave lined with PTFE. After hydrothermal reaction at 120 °C for 12 hours, the solution was cooled to room temperature to obtain a brown mixture. The solid product obtained by centrifugation (10,000 rpm, 5 minutes) was washed three times with water, ethanol, and hexane, respectively, to obtain Cu nanowires. Finally, the Cu nanowires were stored in 8 mL of anhydrous ethanol.

[0082] (2) Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial

[0083] Two mL of freshly synthesized Cu nanowire ethanol dispersion was dispersed in 18 mL of degassed methanol solution containing 200 mg CTAB, and the solution was sonicated for 20 min followed by degassed for 10 min. Then, 54 mg of 2-methylimidazole and 50 mg of Zn(NO3)2·6H2O were dissolved in 5 mL of degassed methanol, respectively. Finally, under nitrogen protection, the methanol solution of 2-methylimidazole and Zn(NO3)2·6H2O were added sequentially to the one-dimensional Cu nanowires dispersed in the organic solvent. The vial was sealed with a diaphragm and left to stand at room temperature for 1 hour without stirring. The suspension was collected by centrifugation under air-free conditions and washed three times with degassed methanol. The solid product was obtained by centrifugation and then vacuum dried overnight at room temperature to obtain the Zn-based MOF-encapsulated one-dimensional Cu nanomaterial Cu NWs@ZIF-8.

[0084] (3) Preparation of one-dimensional Zn / Cu single-atom alloy catalysts

[0085] A one-dimensional Zn / Cu single-atom alloy catalyst was synthesized by direct carbonization of Cu NWs@ZIF-8 prepared in step (2) under an argon flow at 800 °C. The prepared Cu NWs@ZIF-8 was placed in a tube furnace and heated to 20 mL min. –1 At an argon flow rate of 5℃ / min –1 The sample was heated to 800°C for 2 hours at a heating rate of [missing information]. After calcination, the sample was cooled to room temperature to obtain a one-dimensional Zn / Cu single-atom alloy catalyst, CuZn / Cu SAAs.

[0086] Example 8: Preparation of one-dimensional Zn / Cu single-atom alloy catalyst

[0087] (1) Construction of one-dimensional Cu nanomaterials:

[0088] A 40 mL aqueous solution containing 85 mg CuCl₂·2H₂O, 500 mg HDA, and 111 mg D-(+)-glucose was vigorously stirred overnight at 45 °C to obtain a light blue emulsion mixture, which was then sonicated for 20 minutes. The solution was transferred to a 100 mL stainless steel autoclave lined with PTFE. After hydrothermal reaction at 120 °C for 12 hours, the solution was cooled to room temperature to obtain a brown mixture. The solid product obtained by centrifugation (10,000 rpm, 5 minutes) was washed three times with water, ethanol, and hexane, respectively, to obtain Cu nanowires. Finally, the Cu nanowires were stored in 8 mL of anhydrous ethanol.

[0089] (2) Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial

[0090] Two mL of freshly synthesized Cu nanowire ethanol dispersion was dispersed in 18 mL of degassed methanol solution containing 200 mg CTAB, and the solution was sonicated for 20 min followed by degassed for 10 min. Then, 54 mg of 2-methylimidazole and 50 mg of Zn(NO3)2·6H2O were dissolved in 5 mL of degassed methanol, respectively. Finally, under nitrogen protection, the methanol solution of 2-methylimidazole and Zn(NO3)2·6H2O were added sequentially to the one-dimensional Cu nanowires dispersed in the organic solvent. The vial was sealed with a diaphragm and left to stand at room temperature for 1 hour without stirring. The suspension was collected by centrifugation under air-free conditions and washed three times with degassed methanol. The solid product was obtained by centrifugation and then vacuum dried overnight at room temperature to obtain the Zn-based MOF-encapsulated one-dimensional Cu nanomaterial Cu NWs@ZIF-8.

[0091] (3) Preparation of one-dimensional Zn / Cu single-atom alloy catalysts

[0092] A one-dimensional Zn / Cu single-atom alloy catalyst was synthesized by direct carbonization of Cu NWs@ZIF-8 prepared in step (2) under an argon flow at 800 °C. The prepared Cu NWs@ZIF-8 was placed in a tube furnace and heated to 20 mL min. –1 At an argon flow rate of 5℃ / min –1 The sample was heated to 800°C for 3 hours at a specific heating rate. After calcination, the sample was cooled to room temperature to obtain a one-dimensional Zn / Cu single-atom alloy catalyst, CuZn / Cu SAAs.

Claims

1. An application of a one-dimensional Zn / Cu single-atom alloy catalyst, characterized in that, The catalyst is used in the thermocatalytic hydrogenation of CO2 to produce methanol, and the preparation steps of the catalyst are as follows: Step 1, Construction of one-dimensional Cu nanomaterials: The Cu precursor solution was heated and stirred, and then subjected to ultrasonication, hydrothermal reaction, centrifugation, and washing in sequence to obtain Cu nanowires; Step 2, Construction of Zn-based MOF layer on surface of one-dimensional Cu nanomaterial: The one-dimensional Cu nanowires obtained in step 1 are dispersed in an organic solvent, sonicated and degassed, and the degassed organic ligand solution and Zn(NO3)2 solution are added in sequence. After standing for 1-2 hours, the one-dimensional Cu nanomaterials are obtained by centrifugation and washing. Step 3, Preparation of one-dimensional Zn / Cu single-atom alloy catalyst: The one-dimensional Cu nanomaterials wrapped with Zn-based MOF obtained in step 2 are calcined in an inert atmosphere at high temperature to obtain the one-dimensional Zn / Cu single-atom alloy catalyst. The prepared catalyst was used for the thermocatalytic hydrogenation of CO2 to methanol, and the methanol selectivity reached 100% in the range of 150~210℃.

2. The application according to claim 1, characterized in that: The heating and stirring temperature in step 1 is 45-50℃.

3. The application according to claim 1, characterized in that: The organic solvent is 0.028-0.032 mol / mL. -1 A methanol solution of CTAB.

4. The application according to claim 1, characterized in that: The organic ligand solution is a methanol solution of 2-methylimidazole.

5. The application according to claim 4, characterized in that: The mass ratio of 2-methylimidazole to Zn(NO3)2 is 1~1.

2.

6. The application according to claim 1, characterized in that: The hydrothermal reaction conditions are 115-125℃ for 11.8-13 hours.

7. The application according to claim 1, characterized in that: The inert atmosphere is argon, and the inlet gas flow rate is 15-25 mL / min. –1 High-temperature calcination conditions are 2-5℃ min. –1 Heat to 800℃ for 2-3 hours at the specified heating rate.

Citation Information

Patent Citations

  • Preparation method of copper nanowire-metal organic framework core-shell composite material

    CN113845777A