A wear-resistant transparent super-hydrophilic surface and a preparation method and application thereof

By preparing TiN, TiC, or TiCN layers on a transparent substrate and constructing a porous micro/nano structure coating, the problem of insufficient wear resistance and hydrophilicity of titanium dioxide coatings under visible light is solved, realizing the preparation of a wear-resistant, transparent, and superhydrophilic surface, which is suitable for the field of anti-fogging in optical lenses.

CN118108419BActive Publication Date: 2026-11-24NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211514292.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-29
Publication Date
2026-11-24
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

Existing titanium dioxide coatings cannot maintain their superhydrophilic anti-fog effect for a long time under visible light, and their wear resistance is insufficient, which limits their application.

Method used

TiN, TiC, or TiCN layers are prepared on a transparent substrate using physical vapor deposition. A porous micro/nano structure coating is constructed by anodic oxidation and then subjected to heat treatment to obtain a wear-resistant, transparent, and superhydrophilic surface.

Benefits of technology

It maintains its super-hydrophilic anti-fog effect under visible light and significantly improves the coating's abrasion resistance and light transmittance, making it suitable for anti-fog applications in optical lenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118108419B_ABST
    Figure CN118108419B_ABST
Patent Text Reader

Abstract

This invention discloses a wear-resistant, transparent, superhydrophilic surface, its preparation method, and its applications. The preparation method of the wear-resistant, transparent, superhydrophilic surface includes: preparing a TiN layer, TiC layer, or TiCN layer on a transparent substrate using physical vapor deposition; anodizing the TiN layer, TiC layer, or TiCN layer to obtain a coating with a porous micro / nano structure; and heat-treating the coating with the porous micro / nano structure to obtain the wear-resistant, transparent, superhydrophilic surface. The wear-resistant, transparent, superhydrophilic surface obtained by this invention exhibits a light transmittance decrease of no more than 3% compared to the original transparent substrate, a water contact angle ≤10°, and a contact angle still ≤10° after 100 cycles of friction with a 1KG load on nonwoven fabric. This invention is simple, widely applicable, and has broad application prospects in fields such as anti-fogging of optical lenses.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional materials technology, specifically relating to a wear-resistant, transparent, superhydrophilic surface, its preparation method, and its application. Background Technology

[0002] Superhydrophilic surfaces exhibit strong wettability to water, making them promising for applications in anti-fogging and heat dissipation. Anti-fogging applications require high transparency, and long-term use also demands high surface abrasion resistance. While titanium dioxide films exhibit superhydrophilicity under ultraviolet light, this anti-fogging effect only lasts for a few hours to about a week, reverting to a hydrophobic state after UV exposure. The need for frequent UV exposure to maintain its hydrophilicity severely limits the application of titanium dioxide coatings. Therefore, developing a coating based on titanium dioxide that maintains superhydrophilic anti-fogging properties under visible light, while also possessing abrasion resistance and high transparency, is of paramount importance. Summary of the Invention

[0003] The main objective of this invention is to provide a wear-resistant, transparent, superhydrophilic surface, its preparation method, and its application, in order to overcome the shortcomings of the prior art.

[0004] To achieve the aforementioned objectives, the technical solution adopted by this invention includes:

[0005] This invention provides a method for preparing a wear-resistant, transparent, superhydrophilic surface, comprising:

[0006] TiN, TiC, or TiCN layers are prepared on transparent substrates using physical vapor deposition.

[0007] Anodizing of TiN, TiC, or TiCN layers yields coatings with porous micro / nano structures.

[0008] The wear-resistant, transparent, superhydrophilic surface is obtained by heat-treating a coating with a porous micro / nano structure.

[0009] Furthermore, the thickness of the TiN layer, TiC layer, or TiCN layer is 50–500 nm.

[0010] Furthermore, the surface roughness of the porous micro / nano structure coating is 20–100 nm, and the pore size of the porous micro / nano structure coating is 10–100 nm.

[0011] This invention also provides a wear-resistant, transparent, superhydrophilic surface prepared by the aforementioned method. Compared with the original transparent substrate, the light transmittance of the wear-resistant, transparent, superhydrophilic surface decreases by no more than 3%, the water contact angle is ≤10°, and the contact angle is still ≤10° after 100 cycles of friction with a 1KG load nonwoven fabric.

[0012] This invention also provides the application of the aforementioned wear-resistant, transparent, superhydrophilic surface in the field of anti-fogging for optical lenses.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] This invention employs physical vapor deposition (PVD) to prepare a wear-resistant underlayer of TiN, TiC, or TiCN. Then, anodizing is used to construct a metal oxide layer with a micro / nano structure, followed by heat treatment for phase transformation modification. This results in a superhydrophilic coating surface with excellent wear resistance and light transmittance. Furthermore, the method of this invention is simple, can be mass-produced, and is inexpensive, making it a promising candidate for industrial applications. Attached Figure Description

[0015] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0016] Figure 1 This is a morphology diagram of the wear-resistant, transparent, superhydrophilic surface prepared in Example 1 of this invention.

[0017] Figure 2 This is a schematic diagram of the contact angle of the wear-resistant, transparent, superhydrophilic surface prepared in Embodiment 1 of the present invention.

[0018] Figure 3 This is a schematic diagram of the contact angle of the wear-resistant, transparent, superhydrophilic surface prepared in Example 1 of the present invention after being rubbed 100 times with a nonwoven fabric under a 1KG load.

[0019] Figure 4 This is a schematic diagram of the light transmittance of the wear-resistant, transparent, superhydrophilic surface prepared in Example 1 of the present invention.

[0020] Figure 5 This is a schematic diagram of the contact angle of the coating surface prepared in Comparative Example 1.

[0021] Figure 6 This is a schematic diagram of the contact angle of the coating surface prepared in Comparative Example 2. Detailed Implementation

[0022] The invention will be more fully understood through the following detailed description, which should be read in conjunction with the accompanying drawings. Detailed embodiments of the invention are disclosed herein; however, it should be understood that the disclosed embodiments are merely exemplary of the invention, which may be embodied in various forms. Therefore, the specific functional details disclosed herein should not be construed as limiting, but rather as the basis for the claims and as intended to teach those skilled in the art to employ the representative basis of the invention in different ways in any suitable detailed embodiment.

[0023] In view of the deficiencies of the prior art, the inventors of this case, through long-term research and extensive practice, have proposed the technical solution of this invention. The technical solution of this invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0024] One aspect of this invention provides a method for preparing a wear-resistant, transparent, superhydrophilic surface, comprising:

[0025] TiN, TiC, or TiCN layers are prepared on transparent substrates using physical vapor deposition.

[0026] Anodizing of TiN, TiC, or TiCN layers yields coatings with porous micro / nano structures.

[0027] The wear-resistant, transparent, superhydrophilic surface is obtained by heat-treating a coating with a porous micro / nano structure.

[0028] In some preferred embodiments, the thickness of the TiN layer, TiC layer, or TiCN layer is 50–500 nm.

[0029] In some preferred embodiments, the surface roughness of the porous micro / nano structure coating is 20–100 nm, and the pore size of the porous micro / nano structure coating is 10–100 nm.

[0030] In some preferred embodiments, the method for preparing the wear-resistant transparent superhydrophilic coating includes: placing a transparent substrate in the vacuum chamber of a coating equipment, and depositing a TiN, TiC, or TiCN layer on the transparent substrate using magnetron sputtering or multi-arc ion plating technology.

[0031] In some more preferred embodiments, the process conditions for the magnetron sputtering technology include: a DC magnetron power supply controlling the Ti target, a target current of 2A to 7A, a deposition bias of -100V to -400V, a deposition temperature of 50℃ to 200℃, a deposition pressure of 0.3 to 1Pa, a rotary table speed of 1rpm to 5rpm, and working gases including argon, nitrogen, and acetylene; the conditions for depositing the TiN layer include: an argon flow rate of 40sccm to 100sccm, a nitrogen flow rate of 20 to 60sccm, and a deposition time of 2min to 30min; the conditions for depositing the TiC layer include: an argon flow rate of 50-80sccm, an acetylene flow rate of 10sccm to 100sccm, and a deposition time of 1min to 60min; and the conditions for depositing the TiCN layer include: an argon flow rate of 50-80sccm, a nitrogen flow rate of 20-60sccm, an acetylene flow rate of 10sccm to 100sccm, and a deposition time of 1min to 30min.

[0032] In some more preferred embodiments, the preparation method includes: first cleaning, degreasing, and surface activation treatment of the transparent substrate, and then forming the TiN, TiC, or TiCN layer on the substrate using magnetron sputtering technology; wherein, the activation treatment includes: placing the substrate in the vacuum chamber of the coating equipment, evacuating the vacuum chamber, raising the temperature inside the vacuum chamber to 80℃~200℃, introducing argon gas, turning on the ion beam with an ion beam voltage of 1000V-1300V to increase the gas ionization rate, and applying a bias voltage of -200V~-500V to the metal substrate, thereby guiding argon ions to bombard and activate the metal surface.

[0033] In some more preferred embodiments, the multi-arc ion plating technique for depositing TiN, TiC, or TiCN layers includes the following steps:

[0034] S1. The transparent substrate was ultrasonically cleaned for 10 minutes with petroleum ether, acetone or alcohol, respectively. Finally, the sample surface was cleaned with deionized water and the sample was dried with a nitrogen gun.

[0035] S2. Place the washed sample into the deposition chamber and evacuate to a vacuum level of 3 × 10⁻⁶. -5 Pa ~ 7×10 -5 Pa, while being heated, with a heating temperature of 350℃~450℃;

[0036] S3. Perform ion etching on the sample, cleaning with Ar ions at substrate negative bias voltages of -900V, 1100V, and 1200V for 2–10 min.

[0037] S4. Preparation of TiN, TiC, or TiCN coatings, wherein the process conditions for the coating include: Ti target current of 60A to 80A; deposition bias of -20V to -300V; deposition temperature of 300℃ to 500℃; deposition pressure of 0.3 to 1Pa; rotary table speed of 1rpm to 5rpm; and working gases including argon, nitrogen, and acetylene. The conditions for depositing the TiN layer include: argon flow rate of 200sccm to 400sccm, nitrogen flow rate of 300 to 800sccm, and deposition time of 1min to 10min. The conditions for depositing the TiC layer include: argon flow rate of 200-400sccm, acetylene flow rate of 200sccm to 600sccm, and deposition time of 1min to 5min. The conditions for depositing the TiCN layer include: argon flow rate of 100sccm to 300sccm, nitrogen flow rate of 300-800sccm, acetylene flow rate of 100sccm to 600sccm, and deposition time of 1min to 10min.

[0038] In some more preferred embodiments, the preparation method includes: after forming the TiN or TiC or TiCN layer, reducing the temperature of the vacuum chamber of the coating equipment to below 50°C and then removing the substrate having the TiN or TiC or TiCN layer.

[0039] In practice, during the deposition of the TiN, TiC, or TiCN layer, the coating thickness and composition can be controlled by at least adjusting the flow rates of nitrogen and acetylene and the deposition time.

[0040] In some preferred embodiments, the method for preparing the wear-resistant transparent superhydrophilic coating includes:

[0041] The substrate with a TiN, TiC, or TiCN coating is ultrasonically cleaned and dried.

[0042] The dried TiN, TiC, or TiCN layer substrate is connected to the positive terminal of a DC power supply in an electrolyte, and the counter electrode graphite sheet is connected to the negative terminal of a DC power supply. The coating is anodized under the conditions of voltage of 10V to 50V, current of 0.8A to 2A, temperature of 25℃ to 35℃, and time of 5min to 60min.

[0043] In some more preferred embodiments, the steps and process conditions used for anodizing the TiN, TiC, or TiCN layer are as follows:

[0044] S1. The substrate with deposited TiN, TiC or TiCN layers was ultrasonically cleaned with alcohol and deionized water for 10 min respectively, and finally the sample was dried with a nitrogen gun.

[0045] S2. In an electrolyte, a substrate with a deposited TiN, TiC, or TiCN layer is connected to the positive terminal of a DC power supply, and a graphite sheet as the counter electrode is connected to the negative terminal of a DC power supply. The coating is anodized under the following conditions: voltage 10V to 50V, current 0.8A to 2A, temperature 25℃ to 35℃, and time 5min to 60min. The electrolyte is an ethylene glycol solution containing 0.2wt% to 4wt% NH4F and 1vol% to 5vol% water.

[0046] In some preferred embodiments, the method for preparing the wear-resistant transparent superhydrophilic surface includes: subjecting a substrate sample with a porous micro / nano structure coating formed by anodizing a TiN, TiC, or TiCN layer to heat treatment in a protective atmosphere to improve the crystallinity of the coating, thereby obtaining the wear-resistant transparent superhydrophilic surface.

[0047] In some more preferred embodiments, the protective atmosphere comprises atmosphere and / or a combination of oxygen and an inert gas, wherein the inert gas is selected as argon.

[0048] In some more preferred embodiments, the heat treatment temperature is 400℃~800℃, the heat treatment time is 60min~6h, and the heating rate and cooling rate are 2~10℃ / min.

[0049] Another aspect of the present invention provides a wear-resistant transparent superhydrophilic surface prepared by the aforementioned method, wherein the light transmittance of the wear-resistant transparent superhydrophilic surface decreases by no more than 3% compared with the original transparent substrate, the water contact angle is ≤10°, and the contact angle is still ≤10° after being rubbed 100 times with a nonwoven fabric under a 1KG load.

[0050] This invention also provides the application of the aforementioned wear-resistant, transparent, superhydrophilic surface in the field of anti-fogging for optical lenses.

[0051] The embodiments of this invention employ physical vapor deposition (PVD) to prepare a wear-resistant underlayer of TiN, TiC, or TiCN. Then, anodizing is used to construct a metal oxide layer with a micro / nano structure, followed by heat treatment for phase transformation modification. This results in a superhydrophilic surface and an coating with excellent wear resistance and light transmittance. Furthermore, the method of this invention is simple, can be mass-produced, and is inexpensive, making it a promising candidate for industrial applications.

[0052] The technical solution of the present invention will be further described in detail below with reference to several preferred embodiments and accompanying drawings. This embodiment is implemented on the premise of the technical solution of the invention, and provides detailed implementation methods and specific operation processes. However, the protection scope of the present invention is not limited to the following embodiments.

[0053] Unless otherwise specified, the experimental materials used in the examples below can be purchased from conventional biochemical reagent companies.

[0054] Example 1

[0055] (1) Fabrication of TiN layers by magnetron sputtering

[0056] The glass substrate was placed in the vacuum chamber of the coating equipment, and the vacuum chamber was evacuated. The temperature inside the vacuum chamber was then raised to 200°C, and argon gas was introduced. The ion beam was turned on with a voltage of 1300V to increase the gas ionization rate. A bias voltage of -400V was applied to the metal substrate to guide the argon ions to bombard and activate the metal surface. The film deposition parameters included: Ti target current of 3A, deposition bias voltage of -100V, deposition temperature of 200°C, deposition pressure of 0.6Pa, rotary table speed of 2rpm, argon gas flow rate of 40sccm, nitrogen gas flow rate of 50sccm, deposition time of 5min, and the thickness of the deposited TiN film was 90nm.

[0057] (2) TiN anodizing

[0058] A substrate with a TiN coating was connected to the positive terminal of a DC power supply in an electrolyte, and a graphite sheet was connected to the negative terminal of the DC power supply as the counter electrode. The coating was anodized under the conditions of 20V, 35℃ and 30min. The electrolyte was an ethylene glycol solution containing 4wt% NH4F and 1vol% water.

[0059] (3) Anodizing TiN heat treatment phase transition

[0060] The anodized sample was heat-treated in a muffle furnace under air atmosphere at a temperature of 500℃ for 120 min, with a heating rate and a cooling rate of 5℃ / min.

[0061] Figure 1 This describes the morphology of the wear-resistant, transparent, superhydrophilic surface prepared in Example 1 of this invention; Figure 2 The contact angle (4°) of the wear-resistant transparent superhydrophilic surface prepared in Example 1 of this invention; Figure 3 The contact angle (3°) of the wear-resistant transparent superhydrophilic surface prepared in Example 1 of the present invention after being rubbed 100 times with a nonwoven fabric under a 1KG load; Figure 4 The transmittance (90%) of the wear-resistant, transparent, superhydrophilic surface prepared in Example 1 of this invention.

[0062] Example 2

[0063] (1) Fabrication of TiN layers by magnetron sputtering

[0064] A glass substrate was placed in the vacuum chamber of the coating equipment, and the vacuum chamber was evacuated. The temperature inside the vacuum chamber was then raised to 200°C, and argon gas was introduced. The ion beam was activated with a voltage of 1300V to increase the gas ionization rate. A bias voltage of -400V was applied to the metal substrate to guide the argon ions to bombard and activate the metal surface. The film deposition parameters included: Ti target current of 2A, deposition bias voltage of -100V, deposition temperature of 200°C, deposition pressure of 0.6Pa, rotary table speed of 2rpm, argon gas flow rate of 40sccm, nitrogen gas flow rate of 50sccm, deposition time of 5min, and a deposited TiN film thickness of 50nm.

[0065] (2) TiN anodizing

[0066] A substrate with a TiN coating was connected to the positive terminal of a DC power supply in an electrolyte, and a graphite sheet was connected to the negative terminal of the DC power supply as the counter electrode. The coating was anodized under the conditions of 20V, 35℃ and 10min. The electrolyte was an ethylene glycol solution containing 4wt% NH4F and 1vol% water.

[0067] (3) Anodizing TiN heat treatment phase transition

[0068] The anodized sample was heat-treated in a muffle furnace under air atmosphere at a temperature of 500℃ for 120 min, with a heating rate and a cooling rate of 5℃ / min.

[0069] Example 3

[0070] (1) Fabrication of TiN layers by magnetron sputtering

[0071] A glass substrate was placed in the vacuum chamber of the coating equipment, and the vacuum chamber was evacuated. The temperature inside the vacuum chamber was then raised to 200°C, and argon gas was introduced. The ion beam was activated with a voltage of 1300V to increase the gas ionization rate. A bias voltage of -400V was applied to the metal substrate to guide the argon ions to bombard and activate the metal surface. The film deposition parameters included: Ti target current of 7A, deposition bias voltage of -100V, deposition temperature of 200°C, deposition pressure of 0.6Pa, rotary table speed of 2rpm, argon gas flow rate of 40sccm, nitrogen gas flow rate of 50sccm, deposition time of 5min, and a deposited TiN film thickness of 500nm.

[0072] (2) TiN anodizing

[0073] A substrate with a TiN coating was connected to the positive terminal of a DC power supply in an electrolyte, and a graphite sheet was connected to the negative terminal of the DC power supply as the counter electrode. The coating was anodized under the conditions of 20V, 35℃ and 50min. The electrolyte was an ethylene glycol solution containing 4wt% NH4F and 1vol% water.

[0074] (3) Anodizing TiN heat treatment phase transition

[0075] The anodized sample was heat-treated in a muffle furnace under air atmosphere at a temperature of 500℃ for 120 min, with a heating rate and a cooling rate of 5℃ / min.

[0076] Example 4

[0077] (1) Fabrication of TiC layer by magnetron sputtering

[0078] The glass substrate was placed in the vacuum chamber of the coating equipment, and the vacuum chamber was evacuated. The temperature inside the vacuum chamber was then raised to 200°C, and argon gas was introduced. The ion beam was turned on with a voltage of 1300V to increase the gas ionization rate. A bias voltage of -400V was applied to the metal substrate to guide the argon ions to bombard and activate the metal surface. The film deposition parameters included: Ti target current of 4A, deposition bias voltage of -150V, deposition temperature of 150°C, deposition pressure of 0.3Pa, rotary table speed of 2rpm, argon flow rate of 60sccm, acetylene flow rate of 40sccm, deposition time of 10min, and the thickness of the deposited TiC film was 80nm.

[0079] (2) TiC anodic oxidation

[0080] A substrate with a TiC coating was connected to the positive terminal of a DC power supply in an electrolyte, and a graphite sheet was connected to the negative terminal of the DC power supply as the counter electrode. The coating was anodized under the conditions of 10V, 35℃ and 20min. The electrolyte was an ethylene glycol solution containing 4wt% NH4F and 2vol% water.

[0081] (3) Anodizing TiC heat treatment phase transition

[0082] The anodized sample was heat-treated in a muffle furnace under air atmosphere at a temperature of 450℃ for 180 min, with a heating rate and a cooling rate of 10℃ / min.

[0083] Example 5

[0084] (1) Fabrication of TiCN layer by magnetron sputtering

[0085] The glass substrate was placed in the vacuum chamber of the coating equipment, and the vacuum chamber was evacuated. The temperature inside the vacuum chamber was then raised to 150°C, and argon gas was introduced. The ion beam was turned on with a voltage of 1200V to increase the gas ionization rate. A bias voltage of -300V was applied to the metal substrate to guide the argon ions to bombard and activate the metal surface. The film deposition parameters included: TiAl target current of 3A, deposition bias voltage of -200V, deposition temperature of 150°C, deposition pressure of 0.3Pa, turntable speed of 2rpm, argon gas flow rate of 60sccm, nitrogen gas flow rate of 50sccm, acetylene gas flow rate of 60sccm, deposition time of 5min, and the thickness of the deposited TiCN film was 200nm.

[0086] (2) TiCN anodizing

[0087] A substrate with a TiCN coating was connected to the positive terminal of a DC power supply in an electrolyte, and a graphite sheet was connected to the negative terminal of the DC power supply as the counter electrode. The coating was anodized under the conditions of 30V, 35℃ and 50min. The electrolyte was an ethylene glycol solution containing 4wt% NH4F and 3vol% water.

[0088] (3) Anodizing TiCN heat treatment phase transition

[0089] The anodized sample was heat-treated in a muffle furnace under air atmosphere at a temperature of 550℃ for 90 min, with a heating rate and a cooling rate of 5℃ / min.

[0090] Example 6

[0091] (1) Preparation of TiN layer by multi-arc ion plating

[0092] The transparent substrate was ultrasonically cleaned for 10 minutes each with petroleum ether, acetone, and alcohol, respectively. Finally, the sample surface was rinsed with deionized water and dried with a nitrogen gun. The cleaned sample was then placed inside the deposition chamber, and a vacuum of 7 × 10⁻⁶ was applied. 5 The sample was heated to 450℃ using the Pa method. Ion etching was performed on the sample, followed by cleaning with Ar ions at substrate negative biases of -900V, 1100V, and 1200V for 2 min. The process conditions for preparing the TiN coating included: Ti target current of 60A, deposition bias of -50V, deposition temperature of 450℃, deposition pressure of 0.6Pa, rotary table speed of 3rpm, argon flow rate of 200sccm, nitrogen flow rate of 300sccm, deposition time of 2 min, and a film thickness of 100nm.

[0093] (2) TiN anodizing

[0094] A substrate with a TiN coating was connected to the positive terminal of a DC power supply in an electrolyte, and a graphite sheet was connected to the negative terminal of the DC power supply as the counter electrode. The coating was anodized under the conditions of 20V, 35℃ and 30min. The electrolyte was an ethylene glycol solution containing 4wt% NH4F and 1vol% water.

[0095] (3) Anodizing TiN heat treatment phase transition

[0096] The anodized sample was heat-treated in a muffle furnace under air atmosphere at a temperature of 500℃ for 120 min, with a heating rate and a cooling rate of 5℃ / min.

[0097] Compare with Example 1

[0098] (1) Fabrication of TiN layers by magnetron sputtering

[0099] A glass substrate was placed in the vacuum chamber of the coating equipment, and the vacuum chamber was evacuated. The temperature inside the vacuum chamber was then raised to 200°C, and argon gas was introduced. The ion beam was activated with a voltage of 1300V to increase the gas ionization rate. A bias voltage of -400V was applied to the metal substrate to guide the argon ions to bombard and activate the metal surface. The film deposition parameters included: Ti target current of 3A, deposition bias voltage of -100V, deposition temperature of 200°C, deposition pressure of 0.6Pa, rotary table speed of 2rpm, argon gas flow rate of 40sccm, nitrogen gas flow rate of 50sccm, deposition time of 5min, and a TiN film thickness of 90nm.

[0100] (2) Heat treatment of TiN

[0101] The anodized samples were heat-treated in a muffle furnace under air atmosphere at a temperature of 500℃ for 120 min, with a heating and cooling rate of 5℃ / min. The resulting coating had a contact angle of 44°. Figure 5 ).

[0102] Compare with Example 2

[0103] (1) Fabrication of TiN layers by magnetron sputtering

[0104] The glass substrate was placed in the vacuum chamber of the coating equipment, and the vacuum chamber was evacuated. The temperature inside the vacuum chamber was then raised to 200°C, and argon gas was introduced. The ion beam was turned on with a voltage of 1300V to increase the gas ionization rate. A bias voltage of -400V was applied to the metal substrate to guide the argon ions to bombard and activate the metal surface. The film deposition parameters included: Ti target current of 3A, deposition bias voltage of -100V, deposition temperature of 200°C, deposition pressure of 0.6Pa, rotary table speed of 2rpm, argon gas flow rate of 40sccm, nitrogen gas flow rate of 50sccm, deposition time of 5min, and the thickness of the deposited TiN film was 90nm.

[0105] (2) TiN anodizing

[0106] A substrate with a TiN coating was connected to the positive terminal of a DC power supply in an electrolyte, and a graphite sheet as the counter electrode was connected to the negative terminal of the DC power supply. Anodizing of the coating was performed at 20V, 35℃, and 30min. The electrolyte was an ethylene glycol solution containing 4wt% NH4F and 1vol% water. The resulting coating had a contact angle of 40°. Figure 6 ).

[0107] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.

[0108] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims. Moreover, unless specifically stated otherwise, any use of the terms first, second, etc., does not indicate any order or importance, but is used to distinguish one element from another.

Claims

1. The application of a wear-resistant, transparent, superhydrophilic surface in the field of anti-fogging for optical lenses, characterized in that, The method for preparing the wear-resistant, transparent, superhydrophilic surface includes: TiN, TiC, or TiCN layers are prepared on a transparent substrate by physical vapor deposition, wherein the thickness of the TiN, TiC, or TiCN layers is 50-500 nm. Anodizing of TiN, TiC, or TiCN layers under conditions of 10V–50V, 0.8A–2A, 25℃–35℃, and 5min–60min yields a porous micro / nano structure coating. The surface roughness of the porous micro / nano structure coating is 20–100nm, and the pore size is 10–100nm. The wear-resistant, transparent, and superhydrophilic surface is obtained by heat-treating a coating with a porous micro / nano structure to improve the crystallinity of the coating; wherein the heat treatment temperature is 400℃~800℃, the heat treatment time is 60min~6h, and the heating rate and cooling rate are 2~10℃ / min. The wear-resistant, transparent, super-hydrophilic surface has a light transmittance that decreases by no more than 3% compared to the original transparent substrate, a water contact angle of ≤10°, and a contact angle that remains ≤10° after being rubbed 100 times with a 1KG load on nonwoven fabric.

2. The application according to claim 1, characterized in that, The method for preparing the wear-resistant transparent superhydrophilic surface includes: placing a transparent substrate in the vacuum chamber of a coating equipment, and depositing a TiN layer, a TiC layer, or a TiCN layer on the transparent substrate using magnetron sputtering or multi-arc ion plating technology.

3. The application according to claim 1, characterized in that, The method for preparing the wear-resistant, transparent, superhydrophilic surface includes: The substrate with deposited TiN, TiC, or TiCN layers was ultrasonically cleaned and dried. The dried TiN, TiC, or TiCN layer substrate is connected to the positive terminal of a DC power supply in an electrolyte, and the counter electrode graphite sheet is connected to the negative terminal of a DC power supply for the anodic oxidation.

4. The application according to claim 1, characterized in that, The method for preparing the wear-resistant transparent superhydrophilic surface includes: anolyzing a TiN, TiC, or TiCN layer to form a porous micro / nano structure coating, and then subjecting the substrate sample to the heat treatment in a protective atmosphere to obtain the wear-resistant transparent superhydrophilic surface.

5. The application according to claim 4, characterized in that: The protective atmosphere includes atmospheric and / or a combination of oxygen and an inert gas, wherein the inert gas is argon.

Citation Information

Patent Citations

  • Preparation method of coated glass with self-cleaning and energy-saving functions

    CN101891400A

  • Preparation method of titanium dioxide / titanium nitride composite film with adjustable band gaps

    CN102534531A

  • Solid-liquid compounded wear-resistant antibacterial material based on capillary action as well as preparation method and application thereof

    CN112813392A