A method for recovering scandium and uranium from smelting iron-aluminum slag of laterite nickel ore

By using DY366 extractant and multi-stage extraction, washing, and back-extraction steps, the problem of efficient recovery of scandium and uranium from iron-aluminum slag in laterite nickel ore smelting was solved. Rapid phase separation and low-cost scandium and uranium separation at room temperature were achieved, thus improving the recovery efficiency of scandium and uranium.

CN118109692BActive Publication Date: 2026-11-24JINGMEN GEM NEW MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410230242.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2026-11-24
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

In existing technologies, the recovery of scandium and uranium from iron-aluminum slag in laterite nickel ore smelting is difficult to achieve efficiently. In particular, the scandium extraction rate is low, the back-extraction process requires high temperature and long time, and uranium cannot be recovered simultaneously, which affects the impurity removal effect and phase separation speed of subsequent extraction lines, and is also costly.

Method used

The leachate was extracted using DY366 extractant, and then washed and back-extracted with hydrochloric acid, carbonate and acid solutions. Through multi-stage extraction and back-extraction steps, scandium and uranium were recovered separately, avoiding high-temperature heating and achieving rapid phase separation at room temperature.

Benefits of technology

It achieves efficient separation and recovery of scandium and uranium, with scandium extraction rate of over 96% and uranium extraction rate of over 80%. It reduces the processing volume of the extraction process, reduces the loss of cobalt, nickel and manganese, and achieves rapid phase separation without the need for high-temperature heating, thus reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118109692B_ABST
    Figure CN118109692B_ABST
Patent Text Reader

Abstract

This invention discloses a method for recovering scandium and uranium from iron-aluminum slag in laterite nickel ore smelting, comprising the following steps: acid leaching the iron-aluminum slag in laterite nickel ore smelting to obtain a leachate and a leaching residue; extracting the leachate using DY366 extractant to obtain a raffinate and a first loaded organic phase; washing the first loaded organic phase with a detergent to obtain a nickel-containing washing solution and a second loaded organic phase; back-extracting the second loaded organic phase using a first back-extractant to obtain a uranium-containing back-extractant and a third loaded organic phase; and back-extracting the third loaded organic phase using a second back-extractant to obtain a scandium-containing back-extractant and a blank organic phase. This invention, through acid leaching, extraction, and two-step back-extraction, achieves efficient separation of scandium, uranium, and cobalt, nickel, and manganese from the iron-aluminum slag leachate by eliminating the formation of a solid slag phase during the back-extraction process, shortening the back-extraction time, and accelerating phase separation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal recycling technology, and in particular relates to a method for recovering scandium and uranium from iron-aluminum slag smelting in laterite nickel ore. Background Technology

[0002] Laterite nickel ore contains abundant nickel, cobalt, manganese, iron, and aluminum, as well as trace amounts of scandium and uranium. Due to the variety and high content of impurities, it is difficult to directly recover scandium and uranium. Scandium and uranium typically end up in iron-aluminum slag and MHP products. During the wet recovery of cobalt, nickel, and manganese in MHP, scandium and uranium end up in iron-aluminum slag and the extractant in the P204 impurity removal extraction line. Scandium and uranium in the extractant are difficult to back-extract from the extraction line. High scandium concentration in P204 severely affects the extraction and impurity removal efficiency and phase separation rate of the extraction line.

[0003] Currently, scandium recovery primarily employs organophosphate extractants such as P204, P507, and TBP, followed by alkaline back-extraction to precipitate scandium as hydroxide. This method achieves scandium extraction rates generally above 95%, but the back-extraction process generates a large amount of solids, resulting in extremely slow phase separation of the oil, water, and solid phases. Furthermore, a reaction temperature exceeding 70°C and a reaction time exceeding 30 minutes are required to achieve high scandium back-extraction rates and phase separation speeds. The extractant also requires acid regeneration before recycling. This process is lengthy, involves high reaction temperatures, long back-extraction and phase separation times, high alkali consumption, and high costs. Currently, no suitable process has been found for uranium recovery from laterite nickel ore. Summary of the Invention

[0004] To address the aforementioned problems, the present invention aims to provide a method for recovering scandium and uranium from iron-aluminum slag in laterite nickel ore smelting, thereby solving the problems of high reaction temperature, long back-extraction and phase separation time in current scandium recovery processes, as well as the inability to simultaneously recover uranium.

[0005] To achieve the above objectives, the present invention provides the following technical solution:

[0006] This invention provides a method for recovering scandium and uranium from iron-aluminum slag smelting in laterite nickel ore, comprising the following steps:

[0007] (1) Acid leaching treatment was carried out on the iron-aluminum slag from laterite nickel ore smelting to obtain leaching solution and leaching residue;

[0008] (2) The leachate was extracted using DY366 extractant to obtain raffinate and loaded organic phase 1;

[0009] (3) The first loaded organic phase was washed with detergent to obtain a nickel-containing washing solution and the second loaded organic phase;

[0010] (4) The second supported organic phase is back-extracted using the first back-extracting agent to obtain a uranium-containing back-extracting solution and a third supported organic phase;

[0011] (5) The supported organic phase III is back-extracted using the second back-extracting agent to obtain scandium-containing back-extracting solution and blank organic phase.

[0012] Preferably, in step (1), the liquid-to-solid ratio of the acid leaching treatment is 1 to 3:1, the pH is 1.0 to 3.5, the temperature is 50 to 70°C, and the time is 0.5 to 2 hours; the scandium concentration in the leachate is ≥0.6 g / L.

[0013] Preferably, in step (2), the concentration of the extractant is 10-40%, the ratio of the extractant to the leachate is (0.5-4):1, the extraction reaction temperature is 10-50℃, and the number of extraction stages is 1-10.

[0014] Preferably, the detergent in step (3) is a hydrochloric acid and / or sulfuric acid solution, and the concentration of the detergent is 0.5 to 2N.

[0015] Preferably, the washing conditions in step (3) are: the ratio of the loaded organic phase to the detergent is (1-20):1, the temperature is 10-50℃, and the washing level is 1-10.

[0016] Preferably, in step (4), the first stripping agent is a carbonate and / or bicarbonate solution, and the concentration of the first stripping agent is 1 to 2 mol / L.

[0017] Preferably, in step (4), the ratio of the loaded organic phase II to the first stripping agent is (1-10):1, the stripping reaction temperature is 10-50℃, and the number of stripping stages is 1-10.

[0018] Preferably, the second stripping agent in step (5) is an acid solution of 2 to 10 N, and the acid solution is one or both of sulfuric acid and hydrochloric acid.

[0019] Preferably, the ratio of the supported organic phase III to the second stripping agent is (1-10):1, the stripping reaction temperature is 10-50℃, and the number of stripping stages is 1-10.

[0020] Preferably, the above steps further include mixing the leaching residue obtained in step (1) with the raffinate obtained in step (2) to recover nickel and cobalt.

[0021] The beneficial effects of this invention are:

[0022] (1) The present invention enriches scandium and uranium in the iron-aluminum slag from laterite nickel ore smelting and the iron-removing slag from its MHP refining process by cyclic leaching, and then extracts and recovers scandium and uranium, which greatly reduces the processing volume of the extraction process. The leaching residue after leaching can be leached a second time to recover a cobalt-nickel-manganese solution free of scandium and uranium, thus eliminating the adverse effects of scandium and uranium on the downstream extraction and recovery of cobalt-nickel-manganese.

[0023] (2) The leachate enriched with scandium and uranium can selectively recover scandium and uranium through one-step extraction. The scandium extraction rate is above 96% and the uranium extraction rate is above 80%. Cobalt, nickel and manganese and other metals remain in the raffinate. The loss of cobalt, nickel and manganese is less than 5%. This invention achieves efficient separation of scandium, uranium and cobalt, nickel and manganese in iron and aluminum slag leachate and enables comprehensive recovery and utilization of metal elements.

[0024] (3) The back-extraction process of the extractant used in this invention can be carried out at room temperature without heating. No third phase is generated during the back-extraction process, and the phase separation is fast and efficient.

[0025] (4) In this invention, different stripping agents are used to strip scandium and uranium in the supported organic phase in steps to obtain uranium-containing and scandium-containing stripping solutions respectively. The scandium concentration in the uranium-containing stripping solution is below 5 mg / L, and the uranium concentration in the scandium-containing stripping solution is below 1 mg / L. Attached Figure Description

[0026] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings of the embodiments will be briefly described below.

[0027] Figure 1 This is a flowchart of the method for recovering scandium and uranium from iron-aluminum slag smelting of laterite nickel ore according to the present invention. Detailed Implementation

[0028] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0029] Please see Figure 1 The method for recovering scandium and uranium from iron-aluminum slag in laterite nickel ore smelting provided by the present invention includes the following steps:

[0030] (1) The iron-aluminum slag from laterite nickel ore smelting was acid-leached using sulfuric acid. The liquid-solid ratio of the acid leaching treatment was 1-3:1, the pH was 1.0-3.5, the temperature was 50-70℃, and the time was 0.5-2h, to obtain leachate and leachate residue. The acid leaching process can be repeated multiple times until the scandium concentration in the leachate is ≥0.6g / L.

[0031] (2) The leachate was extracted using DY366 extractant. The concentration of the extractant was 10-40%, the ratio of extractant to leachate was (0.5-4):1, the extraction reaction temperature was 10-50℃, and the number of extraction stages was 1-10. Raffinate and supported organic phase I were obtained. The raffinate contained cobalt, nickel, and manganese, and the supported organic phase I contained scandium and uranium.

[0032] (3) Use hydrochloric acid and / or sulfuric acid solution with a concentration of 0.5 to 2N as detergent to wash the loaded organic phase one, the ratio of the loaded organic phase one to the detergent is (1 to 20): 1, the temperature is 10 to 50℃, the washing level is 1 to 10, to obtain nickel-containing washing solution and loaded organic phase two; the nickel-containing washing solution is added to the leachate for extraction.

[0033] (4) The second organic phase is back-extracted using a carbonate and / or bicarbonate solution with a concentration of 1-2 mol / L as the first back-extracting agent. The ratio of the second organic phase to the first back-extracting agent is (1-10):1. The back-extraction reaction temperature is 10-50℃, and the number of back-extraction stages is 1-10, to obtain a uranium-containing back-extracting solution and a third organic phase. The carbonates include, but are not limited to, sodium carbonate and ammonium carbonate, and the bicarbonates include, but are not limited to, one or more of sodium bicarbonate and ammonium bicarbonate.

[0034] (5) Use an acid solution of 2-10N as the second stripping agent to strip the supported organic phase III. The acid solution is one or two of sulfuric acid and hydrochloric acid. The ratio of the supported organic phase III to the second stripping agent is (1-10):1. The stripping reaction temperature is 10-50℃ and the number of stripping stages is 1-10. Scandium-containing stripping solution and blank organic phase are obtained.

[0035] In some preferred embodiments, step (1) further includes acid leaching of the nickel-cobalt hydroxide refining slag to simultaneously recover scandium and uranium from the nickel-cobalt hydroxide refining slag.

[0036] In some preferred embodiments, the above steps further include mixing the leaching residue obtained in step (1) with the raffinate obtained in step (2) to recover nickel and cobalt, wherein the method for recovering nickel and cobalt is a conventional method in the art.

[0037] This invention employs different scandium and uranium leaching enrichment processes and different types of extractants to enrich scandium and uranium in the leaching solution. After enrichment, the volume of solution required for scandium and uranium extraction is greatly reduced. Simultaneously, scandium and uranium are extracted and back-extracted stepwise at room temperature. No solid residue phase is generated during the back-extraction process. The back-extraction time is short and the phase separation is fast. This invention achieves efficient and low-cost recovery of scandium and uranium elements in the system, avoiding the adverse effects of scandium and uranium enrichment on the downstream cobalt, nickel, and manganese recovery.

[0038] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be described in further detail below.

[0039] Example 1

[0040] (1) The iron-aluminum slag from laterite nickel ore smelting and its MHP refining iron removal slag were mixed with water and sulfuric acid for acid leaching treatment. The acid leaching solution solid ratio was 2:1, pH 3.0, temperature 65℃, leaching for 1 hour, and after filtration, the filtrate was mixed with the iron-aluminum slag and sulfuric acid was added. The acid leaching treatment was continued under the above conditions, and the leaching solution and leaching residue were obtained by filtration.

[0041] (2) The leachate was subjected to four countercurrent extractions at 25°C with 30% DY366 at a ratio of 1.2:1 to obtain the raffinate and the loaded organic phase 1.

[0042] (3) The loaded organic phase I was washed countercurrently for 4 stages at 25°C with 1N sulfuric acid at a ratio of 5:1. After phase separation, nickel-containing washing solution and loaded organic phase II were obtained. The nickel-containing washing solution was added to the leachate for extraction.

[0043] (4) The second organic phase was back-extracted in a 1 mol / L ammonium bicarbonate solution at 25°C in a 4:1 ratio for 3 stages. After phase separation, uranium-containing back-extracting solution and the third organic phase were obtained.

[0044] (5) The loaded organic phase was subjected to three countercurrent back-extractions at 25°C with a 4N sulfuric acid solution at a ratio of 10:1 for three stages. After phase separation, scandium-containing back-extraction solution and blank organic phase were obtained.

[0045] Based on the above conditions, the concentrations of major metals in the leachate, raffinate, uranium-containing back-extraction solution, and scandium-containing back-extraction solution are shown in Table 1 below:

[0046] Table 1. Concentrations of major metals in each solution (unit: g / L)

[0047] Main elements Ni Co Mn Sc U Fe leachate 33.1 2.53 2.59 0.6 0.29 0.038 residual liquid 31 2.12 2.47 0.014 0.026 0.002 Uranium-containing back-extraction solution 0.065 0.003 0.002 0.004 0.75 0.001 Scandium-containing back-extraction solution 0.25 0.001 0.001 5.56 0.001 0.21

[0048] Example 2

[0049] (1) The iron-aluminum slag from laterite nickel ore smelting and its MHP refining iron removal slag were mixed with water and sulfuric acid for acid leaching treatment. The acid leaching solution solid ratio was 3:1, pH 2.0, temperature 60℃, leaching for 1.5h, and after filtration, the filtrate was mixed with the iron-aluminum slag and sulfuric acid was added. The acid leaching treatment was carried out under the above conditions, and the leaching solution and leaching residue were obtained by filtration.

[0050] (2) The leachate was subjected to countercurrent extraction with 20% DY366 at 35°C at a ratio of 1.4:1 for 6 stages to obtain the raffinate and the loaded organic phase 1.

[0051] (3) The loaded organic phase I was washed countercurrently for 5 stages at 35°C with 0.5N hydrochloric acid at a ratio of 4:1. After phase separation, nickel-containing washing solution and loaded organic phase II were obtained. The nickel-containing washing solution was added to the leachate for extraction.

[0052] (4) The second organic phase was back-extracted in 1.5 mol / L ammonium bicarbonate solution at 45°C in a 3:1 ratio for 3 stages. After phase separation, uranium-containing back-extracting solution and the third organic phase were obtained.

[0053] (5) The loaded organic phase was subjected to three countercurrent back-extractions at 35°C with 2N sulfuric acid solution at a ratio of 5:1 for three stages. After phase separation, scandium-containing back-extraction solution and blank organic phase were obtained.

[0054] Based on the above conditions, the concentrations of major metals in the leachate, raffinate, uranium-containing back-extraction solution, and scandium-containing back-extraction solution are shown in Table 2 below:

[0055] Table 2. Concentrations of major metals in each solution (unit: g / L)

[0056] Main elements Ni Co Mn Sc U Fe leachate 54.8 2.14 2.13 1.02 0.42 0.11 residual liquid 49.7 1.82 1.77 0.014 0.036 0.001 Uranium-containing back-extraction solution 0.23 0.005 0.002 0.004 0.91 0.001 Scandium-containing back-extraction solution 0.056 0.002 0.002 2.88 0.001 0.45

[0057] Example 3

[0058] (1) The iron-aluminum slag from laterite nickel ore smelting and its MHP refining iron removal slag were mixed with water and sulfuric acid for acid leaching treatment. The acid leaching solution solid ratio was 1.5:1, pH 4.0, temperature 70℃, and leaching was carried out for 2 hours. After filtration, the filtrate was mixed with the iron-aluminum slag and sulfuric acid was added. The acid leaching treatment was carried out under the above conditions, and the acid leaching solution and leaching residue were obtained by filtration.

[0059] (2) The washing solution was countercurrently extracted with 15% DY366 at 50℃ at a ratio of 2:1 for 4 stages to obtain the raffinate and the loaded organic phase 1.

[0060] (3) The loaded organic phase I was washed countercurrently for 4 stages at 50°C with 1.5N sulfuric acid at a ratio of 7:1. After phase separation, nickel-containing washing solution and loaded organic phase II were obtained. The nickel-containing washing solution was added to the leachate for extraction.

[0061] (4) The second organic phase was back-extracted in a 2 mol / L ammonium bicarbonate solution at 45°C with a 6:1 ratio for 4 stages of countercurrent back-extraction. After phase separation, uranium-containing back-extraction solution and the third organic phase were obtained.

[0062] (5) The loaded organic phase was back-extracted in a countercurrent manner for 4 stages at 45°C with 3N sulfuric acid solution at a ratio of 6:1. After phase separation, scandium-containing back-extraction solution and blank organic phase were obtained.

[0063] Based on the above conditions, the concentrations of major metals in the leachate, raffinate, uranium-containing back-extraction solution, and scandium-containing back-extraction solution are shown in Table 3 below:

[0064] Table 3. Concentrations of major metals in each solution (unit: g / L)

[0065] Main elements Ni Co Mn Sc U Fe leachate 32.7 2.65 2.64 1.15 0.35 0.001 residual liquid 28.5 2.43 2.51 0.0008 0.013 0.001 Uranium-containing back-extraction solution 0.18 0.005 0.003 0.003 1.02 0.001 Scandium-containing back-extraction solution 0.044 0.001 0.002 3.54 0.001 0.017

[0066] In summary, this invention first acid-leaches scandium and uranium from iron-aluminum slag, and the enriched leaching residue can then be used to recover nickel and cobalt. A novel extractant is then used to selectively extract scandium and uranium from the leaching solution, while cobalt and nickel remain in the raffinate and can be recovered. Subsequently, a two-stage back-extraction process is used to separate scandium and uranium, resulting in a low-scandium uranium-containing back-extraction solution and a scandium-free back-extraction solution, respectively, thus achieving comprehensive utilization of metallic elements in laterite nickel ore.

[0067] It should be noted that all the above embodiments belong to the same inventive concept, and the descriptions of each embodiment have different focuses. Where the description in a particular embodiment is not detailed, please refer to the description in other embodiments.

[0068] The embodiments described above are merely illustrative of implementation methods of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A method for recovering scandium and uranium from iron-aluminum slag smelting from laterite nickel ore, characterized in that, Includes the following steps: (1) Acid leaching treatment was carried out on the iron-aluminum slag from laterite nickel ore smelting to obtain leaching solution and leaching residue; (2) The leachate was extracted using DY366 extractant to obtain raffinate and loaded organic phase 1; (3) The first loaded organic phase is washed with detergent to obtain a nickel-containing washing solution and a second loaded organic phase; (4) The second supported organic phase is back-extracted using the first back-extracting agent to obtain a uranium-containing back-extracting solution and a third supported organic phase; (5) The supported organic phase III is back-extracted using a second back-extracting agent to obtain a scandium-containing back-extractant and a blank organic phase; In step (4), the first stripping agent is a carbonate and / or bicarbonate solution, and the concentration of the first stripping agent is 1~2 mol / L; In step (5), the second stripping agent is an acid solution of 2~10N, wherein the acid solution is one or both of sulfuric acid and hydrochloric acid.

2. The method for recovering scandium and uranium from iron-aluminum slag smelting from laterite nickel ore according to claim 1, characterized in that, The liquid-to-solid ratio of the acid leaching treatment in step (1) is 1~3:1, the pH is 1.0~3.5, the temperature is 50~70℃, and the time is 0.5~2h; the scandium concentration in the leachate is ≥0.6 g / L.

3. The method for recovering scandium and uranium from iron-aluminum slag smelting from laterite nickel ore according to claim 1, characterized in that, The concentration of the extractant in step (2) is 10~40%, the ratio of extractant to leachate is (0.5~4):1, the extraction temperature is 10~50℃, and the number of extraction stages is 1~10.

4. The method for recovering scandium and uranium from iron-aluminum slag smelting of laterite nickel ore according to claim 1, characterized in that, The detergent in step (3) is a hydrochloric acid and / or sulfuric acid solution, and the concentration of the detergent is 0.5~2N.

5. The method for recovering scandium and uranium from iron-aluminum slag smelting from laterite nickel ore according to claim 1, characterized in that, The washing conditions described in step (3) are: the ratio of the loaded organic phase to the detergent is (1~20):1, the temperature is 10~50℃, and the washing level is 1~10.

6. The method for recovering scandium and uranium from iron-aluminum slag smelting of laterite nickel ore according to claim 1, characterized in that, In step (4), the ratio of the second loaded organic phase to the first stripping agent is (1~10):1, the stripping temperature is 10~50℃, and the number of stripping stages is 1~10.

7. The method for recovering scandium and uranium from iron-aluminum slag smelting from laterite nickel ore according to claim 1, characterized in that, In step (5), the ratio of the supported organic phase III to the second stripping agent is (1~10):1, the stripping temperature is 10~50℃, and the number of stripping stages is 1~10.

8. The method for recovering scandium and uranium from iron-aluminum slag smelting of laterite nickel ore according to claim 1, characterized in that, It also includes recovering nickel and cobalt by mixing the leaching residue obtained in step (1) with the raffinate obtained in step (2).

Citation Information

Patent Citations

  • Method for recycling scandium from lateritic nickel ore smelted iron aluminum slag

    CN103468979A