Application of long-life, multi-reusable piezoelectric single crystal in piezoelectric catalysis field

By using a long-life piezoelectric single-crystal catalyst, the piezoelectric effect under ultrasonic conditions is used to generate active groups to degrade organic dyes, solving the problems of stability and recovery of existing catalysts and achieving efficient and stable treatment of organic wastewater.

CN118122308BActive Publication Date: 2026-11-24SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410172507.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-07
Publication Date
2026-11-24
Estimated Expiration
2044-02-07

AI Technical Summary

Technical Problem

Existing piezoelectric catalysts have low piezoelectric coefficients and poor chemical stability. Furthermore, powdered catalysts suffer from poor stability, difficulty in separation/recovery, and particle agglomeration, which limits their application in organic wastewater treatment.

Method used

Long-life, reusable piezoelectric single crystals, such as lithium niobate and lithium tantalate single crystals, are used. Hydroxyl radicals and superoxide anions are generated through the piezoelectric effect under ultrasonic conditions to attack dye molecules. The single crystals are grown by the Czochralski method to improve stability and facilitate recycling.

Benefits of technology

It achieves efficient degradation of organic dyes, the catalyst's stability does not decay after hundreds of cycles, separation/recovery is easy, particle agglomeration is avoided, and it has a promising application prospect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118122308B_ABST
    Figure CN118122308B_ABST
Patent Text Reader

Abstract

This invention provides an application of a long-life, reusable piezoelectric single crystal in the field of piezoelectric catalysis. The piezoelectric single crystal described in this invention exhibits no stability degradation after hundreds of piezoelectric ultrasonic catalytic degradation cycles, demonstrating promising application prospects in the field of piezoelectric catalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalysts, and in particular relates to the application of a long-life, reusable piezoelectric single crystal in the field of piezoelectric catalysis. Background Technology

[0002] With the rapid development of industrial society and science and technology, environmental pollution, especially water pollution, has become a major obstacle to human health, economic and social sustainable development. Industrial wastewater contains a large amount of organic pollutants, which are toxic and chemically stable. Developing efficient and environmentally friendly water pollution treatment methods has become one of the most prominent and challenging research areas. It has been reported that technologies such as adsorption, chemical oxidation, electrolysis, biotechnology, and photocatalysis have been applied to the degradation of organic pollutants in wastewater. Unfortunately, most of these technologies have some drawbacks, such as high cost, difficulty in completely removing pollutants, and long treatment times, making them ineffective methods for treating organic wastewater. Efficient and environmentally friendly piezoelectric and pyroelectric catalysis are ideal methods for the catalytic degradation of organic pollutants in wastewater.

[0003] Piezoelectric-pyroelectric catalysis involves the release of free electrons and holes from the catalyst surface when subjected to external mechanical vibration (ultrasound, stirring, physical bending, etc.) or temperature changes, thereby initiating a redox reaction in water and further degrading organic pollutants. In recent years, novel piezoelectric-pyroelectric catalysis technologies have shown great application potential and attracted widespread attention. However, currently reported piezoelectric catalysts have relatively low piezoelectric coefficients (3-10). 5 The development of piezoelectric catalysts is limited by their poor chemical stability, particularly those containing pC / N or harmful substances (such as Pb in PZT). Therefore, developing novel piezoelectric materials is an urgent challenge. To date, several piezoelectric materials, such as MoSe2, MoS2, and PbZrO3, have been discovered and widely used as catalysts for the catalytic degradation of organic wastewater. Most existing reports involve catalysts in powder form (micro / nanoparticles). These catalysts suffer from poor stability, difficulties in separation / recovery, and particle agglomeration. Besides powdered catalysts, large-size piezoelectric / ferroelectric crystals are promising catalysts due to their excellent piezoelectric and pyroelectric properties, and more importantly, their recyclability. Summary of the Invention

[0004] In view of this, the present invention aims to propose an application of a long-life, reusable piezoelectric single crystal in the field of piezoelectric catalysis, so as to enable the application of existing piezoelectric single crystals in the field of piezoelectric catalysis.

[0005] To achieve the above objectives, the technical solution of the present invention is implemented as follows:

[0006] Application of a long-life, reusable piezoelectric single crystal in the field of piezoelectric catalysis.

[0007] Hydroxyl radicals (·OH) and superoxide anions (·O2) generated under piezoelectric conditions - They attack dye molecules and break them down into smaller, harmless compounds.

[0008] Preferably, the piezoelectric single crystal is a lithium niobate single crystal and / or a lithium tantalate single crystal.

[0009] Preferably, the catalysis is carried out under ultrasonic conditions, with an ultrasonic frequency of 20kHz to 5000kHz and an ultrasonic power of 100W to 1000W.

[0010] Preferably, the catalysis is the degradation of organic dyes.

[0011] Preferably, the organic dye is any one of methyl orange dye wastewater, rhodamine B dye wastewater, and methylene blue dye wastewater.

[0012] Preferably, the method for preparing the piezoelectric single crystal includes the following steps:

[0013] Step 1: Grind and mix the lithium source and metal compound in a ratio of (50-60):(40-50), pre-calcine at 800℃-900℃ for 2 hours, and then sinter at 1100℃-1200℃ for 3-5 hours to generate polycrystalline material;

[0014] Step 2: Heat the polycrystalline material obtained in Step 1 to 1200℃-1300℃ and keep it at that temperature for 1h-3h to allow the polycrystalline material to fully melt and mix.

[0015] Step 3: Grow single crystals using the Czochralski method;

[0016] Step 4: After the pulling process is completed, the crystal is removed from the liquid surface by heating and melting, and then cooled to room temperature to obtain the final product.

[0017] Preferably, in step one, the lithium source is selected from lithium carbonate.

[0018] Preferably, in step one, the metal compound is selected from niobium pentoxide or tantalum pentoxide.

[0019] Preferably, in step two, the temperature is raised to 1250°C and held at that temperature for 3 hours to allow the lithium niobate polycrystalline material to fully melt and mix.

[0020] Preferably, in step three, the pulling speed is 0.1-0.3 mm / h and the rotation speed is 1-10 r / min. Excessive pulling speed leads to poor crystallinity; insufficient pulling speed affects crystal growth efficiency.

[0021] Preferably, in step three, the lifting speed is 0.3 mm / h and the rotation speed is 5 r / min.

[0022] Preferably, in step four, the cooling rate is 50℃ / h-70℃ / h. This cooling rate makes it easier to grow single crystals with good crystallinity. If the cooling rate is too high, the grown crystal is prone to cracking; if the cooling rate is too low, it affects the crystal growth efficiency.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The piezoelectric single crystal described in this invention has high piezoelectric activity and excellent stability. Its stability did not decay after hundreds of piezoelectric ultrasonic catalytic degradations. At the same time, this type of catalyst is very easy to separate / recover and does not have problems such as particle agglomeration. It has a bright application prospect in the field of piezoelectric catalysis. Attached Figure Description

[0025] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:

[0026] Figure 1 The image shows the XRD pattern of the doped piezoelectric LiNbO3 single crystal described in Example 1 of this invention.

[0027] Figure 2 (a) Ultraviolet-visible absorbance of MB under ultrasonic vibration Figure 2 (b) UV-Vis absorbance of RhB under ultrasonic vibration Figure 2 (c) UV-Vis absorbance of MO under ultrasonic vibration Figure 2 (d) Recovery experiment of RhB degraded by LN. Detailed Implementation

[0028] Unless otherwise defined, the technical terms used in the following embodiments have the same meanings as commonly understood by those skilled in the art. Unless otherwise specified, the experimental reagents used in the following embodiments are conventional biochemical reagents; and the experimental methods described are conventional methods.

[0029] The present invention will now be described in detail with reference to the embodiments and accompanying drawings.

[0030] Example 1:

[0031] Step 1: Grind and mix LiCO3:Nb2O5 in a ratio of 58.5 / 41.5, pre-calcine at 850℃ for 2 hours, and then sinter at 1130℃ for 4 hours to produce polycrystalline lithium niobate.

[0032] Step 2: Place the sintered polycrystalline material in a platinum crucible with a diameter of 100 mm, heat it using a medium frequency power supply to 1250℃, and keep it at a constant temperature for 3 hours to allow the raw materials to fully melt and mix.

[0033] Step 3: Lithium niobate single crystals are grown using the Czochralski method, with a pulling speed of 0.3 mm / h and a rotation speed of 5 r / min.

[0034] Step 4: After the lifting process is completed, we use the method of heating and melting to remove the crystal from the liquid surface, and then cool it down to room temperature at a rate of 60℃ / h.

[0035] Example 2:

[0036] Step 1: Grind and mix LiCO3:Ta2O5 in a ratio of 58.5 / 41.5, pre-calcine at 850℃ for 2 hours, and then sinter at 1130℃ for 4 hours to produce polycrystalline lithium tantalate.

[0037] Step 2: Place the sintered lithium tantalate polycrystalline material into a platinum crucible with a diameter of 100 mm, heat it using a medium frequency power supply to 1250℃, and keep it at a constant temperature for 3 hours to allow the raw materials to fully melt and mix.

[0038] Step 3: Lithium tantalate single crystals are grown using the Czochralski method, with a pulling speed of 0.3 mm / h and a rotation speed of 5 r / min.

[0039] Step 4: After the lifting process is completed, we use the method of heating and melting to remove the crystal from the liquid surface, and then cool it down to room temperature at a rate of 60℃ / h.

[0040] Comparative Example 1: Piezoelectric single crystal + gold nanoparticles

[0041] The lithium niobate substrate comprises three layers, from top to bottom: an 800 nm thick lithium niobate single-crystal thin film layer (+Z side facing up), a 100 nm thick ITO layer, and a 0.3 mm thick lithium niobate substrate. Both the lithium niobate single-crystal thin film layer and the lithium niobate substrate are 5 mm * 5 mm lithium niobate ferroelectric single-crystal wafers cut perpendicular to the c-axis. The topmost 800 nm thick lithium niobate single-crystal thin film layer (+Z side facing up) is the sample layer for depositing gold nanoparticles. Its +Z side has optically level surface flatness, and its ferroelectric domains are single-domain structures parallel to the c-axis. A 25 mM chloroauric acid solution is dropped onto the +Z side of the lithium niobate substrate, and then light is emitted at a wavelength of 280-400 nm and an intensity of 20 mW / cm². 2Ultraviolet light was vertically irradiated at a distance of 5-10 mm above a chloroauric acid solution for 10 minutes, causing several nano-gold nanoparticles to be deposited on the +Z facet of lithium niobate, thus forming a nano-gold-lithium niobate composite material. The formed composite material includes a lithium niobate substrate, on which nano-gold nanoparticles are attached. After the nano-gold nanoparticle deposition, the composite material was first rinsed twice with alcohol for 1 minute each time, then rinsed twice with deionized water for 1 minute each time to remove the acid solution and organic matter attached to the composite material, and finally dried with nitrogen. Using the Au-LiNbO3 composite material as a catalyst, methyl orange was degraded by approximately 55% after 120 minutes of near-infrared light irradiation.

[0042] Comparative Example 2: Catalytic degradation of Rhodamine B by lithium niobate nanoparticles

[0043] LiCO3:Nb2O5 was ground and mixed in a 1:1 ratio, and sintered at 900℃ for 2 hours to produce polycrystalline lithium niobate. Using this polycrystalline lithium niobate as a catalyst, RhB was degraded by ultrasonication, achieving a degradation rate of 90% within 10 minutes. After 10 cycles of catalytic degradation experiments, the degradation rate of the lithium niobate nanoparticle catalyst decreased to 60%.

[0044] Application example: The above examples and comparative examples are applied to catalytic applications.

[0045] The piezoelectric catalytic performance of 1×2cm LN crystals prepared in Example 1 was tested, and the catalytic degradation was carried out using three typical organic dyes (MB, RhB, and Mo) in an ultrasonic process. Specific procedures: The three organic dyes were prepared into 5mg L... -1 An aqueous solution of LN was prepared. LN crystals were placed in solutions of three organic dyes and stirred in the dark for 30 minutes to reach adsorption-desorption equilibrium. Then, an ultrasonic catalytic process was performed using an ultrasonic transducer. To monitor the catalytic activity of LN in real time, the absorbance of the organic dyes was measured every 5 minutes using a UV-Vis spectrophotometer.

[0046] The LN catalyst was used as a catalyst in the piezoelectric-pyroelectric catalytic degradation of organic dyes, and the results were as follows: Figure 2 As shown. The absorption spectra of the dye solution change over time, and corresponding photographs of the MB, RhB, and MO degradation solutions are shown in the figure. Figure 2 As shown in Figure ac, the absorption peak intensity decreases sequentially with increasing ultrasound duration. Furthermore, due to... Figure 2 It can be seen that under ultrasonic conditions, the degradation rates of MB, RhB, and MO within 30 min, 10 min, and 30 min are approximately 90%, 91%, and 65%, respectively. Figure 2 As shown in d. After 80 cycles of catalytic testing, the catalytic performance of LN did not weaken and still maintained 89.5% of its catalytic performance.

[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. An application of a long-life, reusable piezoelectric single crystal in the field of piezoelectric catalysis, wherein the piezoelectric single crystal is a lithium niobate single crystal and / or a lithium tantalate single crystal, the catalysis is the degradation of organic dyes, and the preparation method of the piezoelectric single crystal includes the following steps: Step 1: Grind and mix the lithium source and metal compound in a ratio of (50-60):(40-50), pre-calcine at 800℃-900℃ for 2 hours, and then sinter at 1100℃-1200℃ for 3-5 hours to generate polycrystalline material; Step 2: Heat the polycrystalline material obtained in Step 1 to 1200℃-1300℃ and hold it at that temperature for 1-3 hours to allow the polycrystalline material to fully melt and mix. Step 3: Grow single crystals using the Czochralski method; Step 4: After the pulling process is completed, the crystal is removed from the liquid surface by heating and melting, and then cooled to room temperature to obtain the final product; The catalysis is carried out under ultrasonic conditions, with an ultrasonic frequency of 20kHz to 5000kHz and an ultrasonic power of 100W to 1000W.

2. The application of the long-life, reusable piezoelectric single crystal according to claim 1 in the field of piezoelectric catalysis, characterized in that: The organic dye is derived from any one of the following: methyl orange dye wastewater, rhodamine B dye wastewater, and methylene blue dye wastewater.

3. The application of the long-life, reusable piezoelectric single crystal according to claim 1 in the field of piezoelectric catalysis, characterized in that: In step one, the lithium source is selected from lithium carbonate; In step one, the metal compound is selected from niobium pentoxide or tantalum pentoxide.

4. The application of the long-life, reusable piezoelectric single crystal according to claim 1 in the field of piezoelectric catalysis, characterized in that: In step two, the temperature is raised to 1250°C and held for 3 hours to allow the polycrystalline material to fully melt and mix.

5. The application of the long-life, reusable piezoelectric single crystal according to claim 1 in the field of piezoelectric catalysis, characterized in that: In step three, the lifting speed is 0.1-0.3 mm / h and the rotation speed is 1-10 r / min.

6. The application of the long-life, reusable piezoelectric single crystal according to claim 1 in the field of piezoelectric catalysis, characterized in that: In step three, the lifting speed is 0.3 mm / h and the rotation speed is 5 r / min.

7. The application of the long-life, reusable piezoelectric single crystal according to claim 1 in the field of piezoelectric catalysis, characterized in that: In step four, the cooling rate is 50℃ / h-70℃ / h.