Modified TiO2 composite photocatalyst, its preparation method and application in photocatalytic reduction of Cr in soil 6+ in soil
By growing V₂O₅ on TiO₂ nanosheets to form a direct Z-shaped heterojunction, the problem of easy recombination of photogenerated carriers in the photocatalytic reduction of Cr(VI) by TiO₂ photocatalysts was solved, achieving efficient Cr(VI) reduction and improving the light utilization and catalytic efficiency of the catalyst.
Patent Information
- Application Number
- CN202410060651.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-16
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-16
Smart Images

Figure CN118122309B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a photocatalyst, and more particularly to a modified TiO2 composite photocatalyst, its preparation method, and its photocatalytic reduction of Cr in soil. 6+ Applications in [the field]. Background Technology
[0002] Heavy metal ions are non-biodegradable and, once in the environment, can only migrate and change form, not disappear, thus persisting for a long time. With the increasing scale of agricultural and industrial production, the hazards of heavy metals are becoming increasingly serious. Heavy metal pollution of soil is diverse; when heavy metals remain in the soil for extended periods, they will generally degrade the soil quality of the region. According to surveys, approximately 10 million hectares of arable land in my country are contaminated with heavy metals. 2 This has caused enormous economic losses to our country. Heavy metal pollutants (Cu) in the soil... 2+ Zn 2+ Hg 2+ Cr 3+ Cd 2+ Pb 2+ Pollutants (such as those from electromechanical processing, mining wastewater, mineral processing wastewater, smelting, solid waste, and the use of chemicals) mainly enter the soil through processes like electromechanical processing, mining wastewater, mineral processing wastewater, smelting, solid waste, and the use of chemicals. Simultaneously, they disrupt the ecological balance of the soil environment in various forms, including water-soluble forms, carbonate and oxide-bound forms, ion-exchange forms, and organically bound forms. Crop yields decrease due to soil pollution, and pollutants easily accumulate in plants or indirectly enter the bodies of humans and animals through the food chain, posing a threat to human and animal health.
[0003] Cr(VI) possesses inherent properties that make it highly mobile, stable, and difficult to degrade. Furthermore, Cr(VI) is extremely toxic, more than 100 times more toxic than Cr(III), potentially causing skin irritation upon contact with humans, and increasing the risk of genetic diseases and cancer with prolonged exposure. Therefore, finding a friendly and effective method to treat Cr(VI) in soil is crucial for mitigating and controlling environmental pollution. Photocatalysis technology has attracted considerable attention due to its advantages in contaminated soil remediation, including high efficiency, ease of operation, low cost, and no secondary pollution. The principle of photocatalytic remediation of heavy metals in soil relies primarily on the reduction of heavy metal ions through photocatalysis. Theoretically, any metal ion, as long as its reduction potential is more positive than the conduction band of a semiconductor catalyst, can potentially gain excited electrons from its conduction band and undergo reduction.
[0004] Titanium dioxide (TiO2) is a classic semiconductor photocatalyst. Its advantages, such as low cost, high efficiency, and environmental friendliness, make it irreplaceable and a long-standing research hotspot in the field of photocatalysis. However, problems such as easy recombination of photogenerated carriers and low light utilization affect its performance in the photocatalytic reduction of Cr(VI), limiting its widespread application. Furthermore, although there are reports of titanium dioxide being modified with other materials in existing technologies, these titanium dioxide-modified composite materials are not used for the photocatalytic reduction of heavy metal ions. Currently, there are few reports on the efficient catalytic reduction of heavy metal Cr(VI) using titanium dioxide-modified composite materials, and the catalytic efficiency needs further improvement. Summary of the Invention
[0005] Objectives of the Invention: The first objective of this invention is to provide a modified TiO2 composite photocatalyst that improves the photocatalytic performance of titanium dioxide; the second objective of this invention is to provide a method for preparing the modified TiO2 composite photocatalyst; and the third objective of this invention is to provide the application of the modified TiO2 composite photocatalyst in the photocatalytic reduction of Cr(VI) in soil.
[0006] Technical solution: The modified TiO2 composite photocatalyst of the present invention includes a TiO2 nanosheet support and V2O5 grown on the TiO2 nanosheet, wherein the TiO2 nanosheet and V2O5 form a direct Z-shaped heterojunction structure.
[0007] like Figure 1 As shown, due to the difference in work function and Fermi level between TiO2 and V2O5, during the heterostructure construction process, electrons inside TiO2 spontaneously flow into V2O5 at the internal interface contact region, generating band bending and (-)V2O5@(+)TiO2IIEF, forming a direct Z-type heterojunction. Subsequently, the photoexcitation process of TiO2@V2O5 induces generations of photoexcited electrons and holes. In this case, the photoexcited holes of TiO2 are canceled by the photoexcited electrons of V2O5, thereby achieving the enrichment of photoexcited electrons and holes in TiO2 and V2O5 respectively. The TiO2 and V2O5 parts of TiO2@V2O5 can respectively participate in Cr 6+ Reduction and water oxidation achieve a win-win situation. The charge transfer in the direct Z-junction is a highly efficient and sustained method for reducing Cr in TiO2@V2O5. 6+ Key factors.
[0008] The catalyst has a nanoflower-like structure.
[0009] The preparation method of the modified TiO2 composite photocatalyst of the present invention includes the following steps:
[0010] (1) TiCl4 was dissolved in an organic solvent and water was added to carry out a hydrothermal reaction to obtain TiO2 nanosheets;
[0011] (2) The above TiO2 nanosheets were dispersed in isopropanol, and then vanadium triisopropoxy oxide (VOT) was added. The precursor material obtained after hydrothermal reaction was then calcined to obtain the modified TiO2 composite photocatalyst.
[0012] In step (1), titanium tetrachloride is hydrolyzed to generate titanium hydroxide, and during the hydrothermal reaction, titanium hydroxide undergoes a hydrothermal reaction to generate TiO2 nanosheets.
[0013] Preferably, in step (1), the temperature of the hydrothermal reaction is 90-150°C and the reaction time is 4-10h.
[0014] Preferably, in step (1), the volume ratio of TiCl4, solvent and water is 0.5-5:20-150:1-5.
[0015] Preferably, in step (1), the organic solvent is ethylene glycol.
[0016] Preferably, in step (2), the molar ratio of Ti to V is 1-5:1.5-6.
[0017] Preferably, in step (2), the temperature of the hydrothermal reaction is 180-230°C and the time is 8-12 hours.
[0018] Preferably, in step (2), the precursor is calcined at a temperature of 300–350°C for 1.5–3 hours.
[0019] The modified TiO2 composite photocatalyst described in this invention photocatalytically reduces Cr in soil. 6+ Applications in [the field].
[0020] Mechanism of Invention: The modified TiO2 composite photocatalyst prepared in this invention forms a direct Z-shaped heterojunction between TiO2 and V2O5. Vanadium pentoxide (V2O5) is an important transition metal oxide semiconductor, widely used in lithium-ion batteries, gas sensors, optoelectronic devices, and other fields; it is a strong transition metal oxide catalyst with a typical low band gap (~2.3 eV) and exhibits high photocatalytic activity in the visible light region. Combining TiO2 nanosheets with V2O5 nanosheets creates a heterojunction structure with enhanced reaction area, which not only improves the efficiency of utilizing sunlight but also enhances the charge transfer rate and the separation rate of photogenerated carriers.
[0021] In the photocatalytic reduction of Cr(VI), due to the built-in electric field at the interface of the direct Z-type heterojunction, photoexcited electrons in the conduction band of TiO2 spontaneously transfer to the valence band of V2O5, consuming the residual holes in V2O5. This achieves efficient spatial separation of photogenerated electrons and holes, maintaining the system's strongest redox capability and thus enhancing the system's photocatalytic reduction performance of Cr(VI). Furthermore, by utilizing the difference in band structure to suppress the rapid recombination of electron-hole pairs, the utilization rate of light and the adsorption capacity of Cr(VI) are improved, thereby enhancing the photocatalytic reduction capacity of Cr(VI).
[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The modified TiO2 composite photocatalyst forms a direct Z-type heterojunction between V2O5 and TiO2. The photo-excited electrons in the conduction band of TiO2 are spontaneously transferred to the valence band of V2O5, consuming the residual holes in V2O5. This achieves efficient separation of photogenerated electrons and holes in space and maintains the strongest redox ability of the system, thereby improving the photocatalytic reduction performance of the system; (2) The preparation method of the modified TiO2 composite photocatalyst is simple, the raw material cost is low, and the yield is abundant, which has the premise of being able to be put into large-scale production in the future; (3) The modified TiO2 composite photocatalyst can convert Cr(VI) into Cr(III) through light irradiation, and the photocatalytic reduction efficiency of Cr(VI) can reach up to 91%, which is beneficial to significantly reduce the chemical activity and toxicity of Cr in the environment. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of a Z-shaped heterojunction for a modified TiO2 photocatalyst.
[0024] Figure 2 Scanning electron microscope image of the modified TiO2 composite photocatalyst prepared in Example 4;
[0025] Figure 3 and Figure 4 Transmission electron microscopy image of the modified TiO2 composite photocatalyst prepared in Example 4;
[0026] Figure 5 X-ray diffraction pattern of the modified TiO2 composite photocatalyst prepared in Example 4;
[0027] Figure 6 The diagram shows the efficiency of photocatalytic reduction of Cr(VI) in soil by the modified TiO2 composite photocatalysts prepared in Examples 1-4 under xenon lamp irradiation.
[0028] Figure 7 The modified TiO2 composite photocatalyst prepared in Example 4 and the catalysts prepared in Comparative Examples 1-3 are shown in the photocatalytic reduction efficiency of Cr(VI) in soil under xenon lamp irradiation.
[0029] Figure 8 The UV-Vis diffuse reflectance spectrum of the modified TiO2 composite photocatalyst prepared in Example 4;
[0030] Figure 9 and Figure 10 The images show the fluorescence lifetime spectrum and electrochemical impedance spectroscopy of the modified TiO2 composite photocatalyst prepared in Example 4. Detailed Implementation
[0031] The technical solution of the present invention will be further described below with reference to the embodiments.
[0032] Example 1
[0033] The modified TiO2 composite photocatalyst of the present invention is prepared by the following steps:
[0034] (1) Add 1 mL TiCl4 to 20 mL ethylene glycol solution, stir evenly, add 0.5 mL pure water, transfer the completely dissolved mixed solution to a hydrothermal reactor, and carry out a constant temperature thermal reaction at 110 °C for 10 h. After the reaction is completed, wash the obtained product repeatedly with ultrapure water and anhydrous ethanol, centrifuge and vacuum dry to obtain TiO2 nanosheets.
[0035] (2) 20 mg of the prepared TiO2 nanosheets were ultrasonically dispersed in 50 mL of isopropanol for 10 min. 0.1 g of VOT was added to the solution, and the mixture was stirred for 30 min. The solution was then transferred to a hydrothermal reactor and hydrothermally reacted at 180 °C for 12 h. After the reaction, the mixture was allowed to cool naturally to room temperature. The resulting precipitate was separated by centrifugation, washed four times with anhydrous ethanol, and then vacuum dried. The dried precursor material was calcined at 330 °C for 1.5 h to obtain the modified TiO2 composite photocatalyst TV-20.
[0036] Example 2
[0037] The modified TiO2 composite photocatalyst of the present invention is prepared by the following steps:
[0038] (1) Add 5 mL TiCl4 to 150 mL ethylene glycol solution, stir evenly, add 5 mL pure water, transfer the completely dissolved mixture to a hydrothermal reactor, and carry out a constant temperature thermal reaction at 150 °C for 5 h. After the reaction is completed, wash the obtained product repeatedly with ultrapure water and anhydrous ethanol, centrifuge and vacuum dry to obtain TiO2 nanosheets.
[0039] (2) 40 mg of the prepared TiO2 nanosheets were ultrasonically dispersed in 50 mL of isopropanol for 20 min. 0.15 g of VOT was added to the solution, and the mixture was stirred for 25 min. The solution was then transferred to a hydrothermal reactor and hydrothermally reacted at 210 °C for 10 h. After the reaction, the mixture was allowed to cool naturally to room temperature. The resulting precipitate was separated by centrifugation, washed four times with anhydrous ethanol, and then vacuum dried. The dried precursor material was calcined at 300 °C for 2.5 h to obtain the modified TiO2 composite photocatalyst TV-40.
[0040] Example 3
[0041] The modified TiO2 composite photocatalyst of the present invention is prepared by the following steps:
[0042] (1) Add 0.5 mL TiCl4 to 50 mL ethylene glycol solution, stir evenly, add 2 mL pure water, transfer the completely dissolved mixed solution to a hydrothermal reactor, and carry out a constant temperature thermal reaction at 90 °C for 8 h. After the reaction is completed, wash the obtained product repeatedly with ultrapure water and anhydrous ethanol, centrifuge and vacuum dry to obtain TiO2 nanosheets.
[0043] (2) 100 mg of the prepared TiO2 nanosheets were ultrasonically dispersed in 65 mL of isopropanol for 40 min. 0.3 g of VOT was added to the solution, and the mixture was stirred for 40 min. The solution was then transferred to a hydrothermal reactor and hydrothermally reacted at 230 °C for 8 h. After the reaction, the mixture was allowed to cool naturally to room temperature. The resulting precipitate was separated by centrifugation, washed four times with anhydrous ethanol, and then vacuum dried. The dried precursor material was calcined at 350 °C for 3 h to obtain the modified TiO2 composite photocatalyst TV-100.
[0044] Example 4
[0045] The modified TiO2 composite photocatalyst of the present invention is prepared by the following steps:
[0046] (1) Add 1 mL TiCl4 to 30 mL ethylene glycol solution, stir evenly, add 1.5 mL pure water, transfer the completely dissolved mixed solution to a hydrothermal reactor, and carry out a constant temperature thermal reaction at 135 °C for 4 h. After the reaction is completed, wash the obtained product repeatedly with ultrapure water and anhydrous ethanol, centrifuge and vacuum dry to obtain TiO2 nanosheets.
[0047] (2) 60 mg of the prepared TiO2 nanosheets were ultrasonically dispersed in 60 mL of isopropanol for 30 min. 0.2 g of VOT was added to the solution, and the mixture was stirred for 30 min. The solution was then transferred to a hydrothermal reactor and ultrasonically reacted at 200 °C for 10 h. After the reaction, the mixture was allowed to cool naturally to room temperature. The resulting precipitate was separated by centrifugation, washed four times with anhydrous ethanol, and then vacuum dried. The dried precursor material was calcined at 320 °C for 2 h to obtain the modified TiO2 composite photocatalyst TV-60.
[0048] Comparative Example 1
[0049] Based on Example 4, only step (1) was performed to obtain TiO2 nanosheets, while the other conditions remained unchanged.
[0050] Comparative Example 2
[0051] Based on Example 4, step (1) is omitted, and TiO2 nanosheets are not added in step (2). Only V2O5 is synthesized, and the other conditions remain unchanged.
[0052] Comparative Example 3
[0053] This comparative example provides a TiO2 / V2O5 composite photocatalyst and its preparation method. The main difference between this catalyst and that of Example 4 is that this catalyst is type-II. The specific preparation method is as follows:
[0054] (1) 10 mL of tetrabutyl titanate was added to a mixed solution containing 10 mL of alcohol and 3 mL of acetic acid, and the mixture was stirred in a sealed container for 2 h. Then, 1 g of vinylpyrrolidone was added to the solution, and the reaction was continued for 10 h. The resulting solution was transferred to the syringe of an electrospinning machine, and electrospinning was performed at a voltage of 15 kV and a feed rate of 1.8 mL / h. The obtained product was calcined at 500 °C for 4 h to obtain TiO2 nanorods.
[0055] Step (2) is the same as in Example 4, and TiO2 / V2O5 composite photocatalyst is obtained.
[0056] Structural characterization:
[0057] The modified TiO2 composite photocatalyst synthesized in Example 4 was characterized structurally.
[0058] Figure 2 and Figure 3 , 4 The images shown are scanning electron microscope (SEM) and transmission electron microscope (TEM) images of the modified TiO2 composite photocatalyst prepared in Example 4. Figures 2-4 As can be seen, the composite catalyst exhibits a nanosheet-like structure that is bonded together, forming a nanoflower-like morphology. The intuitive morphological structure diagram initially demonstrates the successful composite of the two materials.
[0059] Figure 5 The X-ray diffraction pattern of the modified TiO2 composite photocatalyst prepared in Example 4 is shown below. Figure 5 It can be seen that the characteristic peaks of TiO2 and V2O5 appeared simultaneously in the composite catalyst, which further illustrates the close bonding between the two materials.
[0060] Performance characterization:
[0061] The photocatalytic performance of the modified TiO2 composite photocatalysts synthesized in Examples 1-4 and the catalysts synthesized in Comparative Examples 1-3 was tested.
[0062] Test Method: Using a photocatalytic reactor (Nanjing Xujiang Electromechanical Plant, XPA-8), under irradiation with a 500W Xe lamp, the heavy metal Cr(VI) was reduced to Cr(III) to evaluate the catalytic activity of the prepared photocatalyst. 5.00g of sterilized soil was weighed and mixed with 5mL of 20mg / L potassium dichromate solution. The mixture was placed in a ventilated area for 12 hours to allow moisture to evaporate. Then, 3.0% (by weight) of modified TiO2 photocatalyst was added to the soil sample, and water was added to maintain a soil moisture content of 30%. The soil sample was evenly spread on the surface and adsorbed in the dark for 1 hour. The petri dish was then placed in the effective light area of a sealed photolysis reaction chamber (uniform and constant light intensity) and irradiated with visible light for 6 hours. The dish was turned over every hour to ensure uniform light exposure, and samples were taken to detect the Cr(VI) concentration.
[0063] Figure 6 The graph shows the photocatalytic reduction efficiency of the modified TiO2 composite photocatalysts prepared in Examples 1-4 for heavy metal Cr(VI) in soil under xenon lamp irradiation. The photocatalytic reduction efficiencies of the modified TiO2 composite photocatalysts TV-20, TV-40, TAV-100 and TAV-60 prepared in Examples 1-4 for Cr(VI) within 6 h are 80%, 89%, 87% and 91%, respectively.
[0064] Figure 7 The graph shows the photocatalytic reduction efficiency of the modified TiO2 composite photocatalyst prepared in Example 4 and the catalysts prepared in Comparative Examples 1-3 under xenon lamp irradiation for the reduction of heavy metal Cr(VI) in soil. The modified TiO2 composite photocatalyst prepared in Example 4 exhibits a photocatalytic reduction efficiency of 90% for Cr(VI), demonstrating excellent photocatalytic performance. Under the same experimental conditions as in Example 4, and without sacrificial agents or photosensitizers, the reduction efficiencies of Comparative Examples 1, 2, and 3 were 55%, 64%, and 76%, respectively. The catalytic efficiency of the modified TiO2 composite photocatalysts prepared in Examples 1-4 of this invention is significantly better than that of the catalysts synthesized in Comparative Examples 1-3, indicating that the combination of TiO2 and V2O5 has a very excellent catalytic effect on the catalyst.
[0065] Figure 8The image shows the UV-Vis spectrum of the modified TiO2 composite photocatalyst prepared in Example 4. As can be seen from the image, TiO2 only absorbs ultraviolet light below 400 nm and does not absorb visible light. V2O5 has good absorption of the entire spectrum of light. After modifying the TiO2 photocatalyst with V2O5, the light absorption capacity of the composite material is significantly improved.
[0066] Figure 9 and Figure 10 The images show the fluorescence lifetime spectrum and electrochemical impedance spectroscopy of the modified TiO2 composite photocatalyst prepared in Example 4. Figure 9 As can be seen from the fitting results, the fluorescence lifetimes of TiO2, V2O5, and the composite material are calculated to be 1.60 ns, 7.70 ns, and 8.06 ns, respectively. The composite material exhibits an increased fluorescence lifetime compared to the two monomeric materials, TiO2 and V2O5. Figure 10 It is evident that the composite material exhibits a smaller quist circle radius compared to the two monomeric materials, TiO2 and V2O5, resulting in a significant decrease in impedance. These findings suggest that constructing a Z-shaped heterojunction suppresses the recombination rate of photogenerated electron-hole pairs, thereby improving photocatalytic efficiency.
Claims
1. A modified TiO2 composite photocatalyst, characterized by, It includes a carrier TiO2 nanosheet and V2O5 grown on the TiO2 nanosheet, with the TiO2 nanosheet and V2O5 forming a direct Z-shaped heterojunction structure.
2. The modified TiO2 composite photocatalyst according to claim 1, characterized in that, The catalyst has a nanoflower-like structure.
3. A method for producing the modified TiO2 composite photocatalyst according to claim 1 or 2, characterized by, Includes the following steps: (1) TiCl4 was dissolved in an organic solvent and water was added to carry out a hydrothermal reaction to obtain TiO2 nanosheets; (2) The above TiO2 nanosheets were dispersed in isopropanol, and then triisopropoxyvanadium oxide was added. The precursor material obtained after hydrothermal reaction was then calcined to obtain the modified TiO2 composite photocatalyst.
4. The method for preparing a modified TiO2 composite photocatalyst according to claim 3, characterized by, In step (2), the molar ratio of Ti to V is 1-5:1.5-6.
5. The method for preparing a modified TiO2 composite photocatalyst according to claim 3, characterized by, In step (2), the temperature of the hydrothermal reaction is 180-230°C and the time is 8-12 hours.
6. The method for preparing a modified TiO2 composite photocatalyst according to claim 3, characterized by, In step (2), the precursor is calcined at a temperature of 300-350°C for 1.5-3 hours.
7. The preparation method of the modified TiO2 composite photocatalyst according to claim 3, characterized in that, In step (1), the temperature of the hydrothermal reaction is 90-150℃ and the reaction time is 4-10h.
8. The preparation method of the modified TiO2 composite photocatalyst according to claim 3, characterized in that, In step (1), the volume ratio of TiCl4, solvent and water is 0.5-5:20-150:1-5.
9. The method for preparing the modified TiO2 composite photocatalyst according to claim 3, characterized in that, In step (1), the organic solvent is ethylene glycol.
10. Use of the modified TiO2 composite photocatalyst according to claim 1 or 2 for photocatalytic reduction of Cr(VI) in soil. 6+
Citation Information
Patent Citations
Method for preparing denitration catalyst by hydrothermal method
CN113019356A
Modified TiO2 composite photocatalyst as well as preparation method and application thereof
CN116422332A