Impact-resistant composite material skateboard and preparation method thereof
By using a hybrid combination of multi-layer composite material structure and high-performance fiber on the skateboard, the shortcomings of existing skateboards in terms of impact and deformation are solved, the comprehensive mechanical properties and service life of the skateboard are improved, and better use effects are achieved.
Patent Information
- Application Number
- CN202410552846.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-05-07
AI Technical Summary
Existing sports skateboards are prone to breakage, low impact strength, and cracking during pedaling during use, resulting in a short service life, and the manufacturing process is complex and prone to process problems.
It adopts a multi-layer composite material structure design, including an upper surface friction-resistant layer, an impact-resistant hybrid fiber composite layer and a lower surface accessory assembly layer. It uses a hybrid combination of carbon fiber, aramid fiber, UHMWPE fiber and glass fiber, and is formed through hot pressing molding technology. High strength, high toughness and impact resistant skateboard structure.
It improves the working comfort and service life of the skateboard, enhances the comprehensive mechanical properties of the skateboard, solves the shortcomings of the existing skateboard in terms of impact and deformation, and extends the service life.
Smart Images

Figure CN118124236B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sports equipment, and in particular to an impact-resistant composite material skateboard and a preparation method thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Currently, the sports skateboards on the market are basically made of laminated wood plywood, or made by bonding wood boards and plastic boards with adhesives. The production structure of the products is relatively complex, and process problems such as delamination of laminated materials are prone to occur during the production process. In addition, the finished skateboards are prone to breakage, low impact strength, and cracking during pedaling during use, which seriously affects the use effect and sports experience, and the service life is relatively short.
[0004] Composite materials with fiber as reinforcement materials are increasingly used in sports skateboards. How to effectively utilize the mechanical advantages of composite materials through reasonable structural design to improve the comprehensive mechanical properties and service life of sports skateboard products has become an urgent problem to be solved. Summary of the invention
[0005] In view of this, the present invention provides an impact-resistant composite skateboard and a preparation method thereof. The provided impact-resistant composite skateboard has comprehensive performance advantages such as light weight, high strength, strong impact resistance and deformation resistance, and has good application prospects.
[0006] In a first aspect, the present invention provides an impact-resistant composite skateboard, which comprises, from top to bottom, an upper surface friction-resistant layer, an impact-resistant hybrid fiber composite layer, and a lower surface accessory assembly layer; a high-strength carbon fiber layer is arranged at the core of the impact-resistant hybrid fiber composite layer;
[0007] The upper surface friction-resistant layer is a polyurethane layer; the impact-resistant mixed fiber composite layer is made of aramid fiber or UHMWPE fiber mixed with glass fiber two-dimensional braided fabric reinforced with thermosetting resin; the lower surface accessory assembly layer is made of high-strength carbon fiber reinforced with thermosetting resin; the high-strength carbon fiber layer is made of high-strength carbon fiber mixed with high-modulus carbon fiber two-dimensional braided fabric reinforced with thermosetting resin.
[0008] In a second aspect, the present invention provides a method for preparing the above-mentioned impact-resistant composite skateboard, comprising the following steps:
[0009] The high-strength carbon fiber mixed with high modulus carbon fiber two-dimensional braid pre-impregnated with thermosetting resin is embedded in the middle of the stack of aramid fiber or UHMWPE fiber mixed with glass fiber two-dimensional braid pre-impregnated with thermosetting resin, and hot-pressed to form an impact-resistant hybrid fiber composite layer with a high-strength carbon fiber layer set in the core;
[0010] The upper surface friction-resistant layer and the lower surface accessory assembly layer are respectively pasted on the upper and lower surfaces of the impact-resistant mixed fiber composite layer, and then subjected to secondary hot pressing molding after drying to obtain the product.
[0011] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0012] The impact-resistant composite skateboard of the present invention adopts a multi-layer composite material structure stacking combination. The layered structure retains the original stacking structure of the wooden skateboard structure, and can absorb the impact energy of the board during movement through the coordination of the interfaces between the multi-layer structures; at the same time, the present invention adopts a mixed combination structure of multiple high-performance fibers such as carbon fiber, aramid fiber, UHMWPE fiber and glass fiber, and through reasonable structural design, the comprehensive mechanical properties of multiple fibers such as high strength, high toughness, and impact resistance are brought into play, thereby improving the working comfort and service life of the skateboard. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0014] Figure 1 Schematic diagram of the overall structure of the impact-resistant composite material skateboard of Examples 1 to 4 of the present invention;
[0015] Figure 2 It is a schematic diagram of the structure of the lower surface accessory assembly layer of embodiments 1 to 4 of the present invention;
[0016] Among them, 1. High-strength carbon fiber layer; 2. Impact-resistant mixed fiber composite layer; 3. Upper surface friction-resistant layer; 4. Lower surface accessory assembly layer; 5. Metal embedded parts. DETAILED DESCRIPTION
[0017] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0018] The present invention provides an impact-resistant composite skateboard, which comprises, from top to bottom, an upper surface friction-resistant layer, an impact-resistant hybrid fiber composite layer, and a lower surface accessory assembly layer; a high-strength carbon fiber layer is arranged at the core of the impact-resistant hybrid fiber composite layer;
[0019] The upper surface friction-resistant layer is a polyurethane layer; the impact-resistant mixed fiber composite layer is made of aramid fiber or UHMWPE fiber mixed with glass fiber two-dimensional braided fabric reinforced with thermosetting resin; the lower surface accessory assembly layer is made of high-strength carbon fiber two-dimensional braided fabric reinforced with thermosetting resin; the high-strength carbon fiber layer is made of high-strength carbon fiber mixed with high-modulus carbon fiber two-dimensional braided fabric reinforced with thermosetting resin.
[0020] In the present invention, the friction-resistant layer on the upper surface of the skateboard contacts the sole of the user and is directly subjected to greater pressure and impact force, so it needs to have better friction resistance. The friction-resistant layer on the upper surface of the present invention is a polyurethane layer. The polyurethane material has a high density and high strength, and can withstand greater friction and pressure. Under heavy loads, the scratches and wear on its surface are small; at the same time, the polyurethane material has a smooth surface and high hardness, and can effectively resist wear caused by friction, shear force and other forces, and has a longer service life. In addition, the polyurethane material also has good elasticity and can self-recover. Even under greater wear or strong impact force, it can maintain good wear resistance and is more comfortable.
[0021] The impact-resistant hybrid fiber composite layer is located below the friction-resistant layer on the upper surface. This layer uses a variety of fibers, among which aramid fiber or UHMWPE fiber (ultra-high molecular weight polyethylene fiber) is a tough fiber with good toughness. It can effectively dissipate energy under the impact force of a large load, thereby reducing damage to the skateboard itself; glass fiber has high strength and can play a reinforcing role. Because it is mixed with tough fiber, it can alleviate the defect of brittleness of glass fiber, so that the impact-resistant hybrid fiber composite layer has both high strength and high toughness.
[0022] The present invention arranges a high-strength carbon fiber layer at the core of the impact-resistant mixed fiber composite layer, and the reinforcing fiber is a mixed fiber of high-strength carbon fiber and high-modulus carbon fiber; after the two carbon fibers with different properties are mixed, the deformation resistance of the skateboard is greatly enhanced; at the same time, the layer is arranged at the core of the skateboard, which not only plays an effective reinforcement and anti-deformation role, but also can reduce the fatigue wear of the high-strength carbon fiber layer, and reduce the cost of repair and maintenance of the skateboard.
[0023] The lower surface accessory assembly layer of the present invention is provided with metal embedded parts so as to be connected with auxiliary parts such as wheel brackets of the skateboard.
[0024] In the present invention, the polyurethane material of the polyurethane layer is selected from any one of an MDI type polyurethane material, a TDI type polyurethane material or an NDI type polyurethane material. Among them, the MDI type polyurethane material refers to a polyurethane material prepared using diphenylmethane diisocyanate as a raw material, the TDI type polyurethane material refers to a polyurethane material prepared using toluene diisocyanate as a raw material, and the NDI type polyurethane material refers to a polyurethane material prepared using naphthalene diisocyanate as a raw material.
[0025] In the present invention, the mixing mass ratio of the aramid fiber or UHMWPE fiber to the glass fiber is (2-10): 1. The aramid fiber or UHMWPE fiber is used as the main fiber in the impact-resistant mixed fiber composite layer, and the glass fiber is used as the auxiliary fiber, which together improves the impact resistance of the impact-resistant mixed fiber composite layer.
[0026] In the present invention, the structures of the two-dimensional braids of the impact-resistant hybrid fiber composite layer, the lower surface accessory assembly layer and the high-strength carbon fiber layer are independently selected from any one of plain, twill or satin weaving structures.
[0027] In the present invention, the impact-resistant hybrid fiber composite layer, the high-strength carbon fiber layer and the thermosetting resin of the high-strength carbon fiber layer are independently selected from any one of epoxy resin, phenolic resin, unsaturated polyester resin or urea-formaldehyde resin, and the resin content is 30-60wt%.
[0028] In the present invention, the high-strength carbon fibers of the lower surface accessory assembly layer and the high-strength carbon fiber layer are independently selected from any one of T300, T700, T800 or T1000.
[0029] In the present invention, the mixed mass ratio of the high-strength carbon fiber and the high modulus carbon fiber in the high-strength carbon fiber layer is (1-3):1; the high modulus carbon fiber in the high-strength carbon fiber layer is selected from any one of M40, M55, M60, M40J, M55J or M60J.
[0030] In the present invention, the projection area of the high-strength carbon fiber layer in the direction parallel to the surface of the impact-resistant composite skateboard accounts for 80-95% of the projection area of the impact-resistant hybrid fiber composite layer in the direction parallel to the surface of the impact-resistant composite skateboard.
[0031] In the present invention, the thickness of the upper surface friction-resistant layer is 0.2-1 mm, the thickness of the impact-resistant mixed fiber composite layer is 3-8 mm, the thickness of the lower surface accessory assembly layer is 0.5-1 mm; and the thickness of the high-strength carbon fiber layer is 1-3 mm.
[0032] The present invention also provides a method for preparing the impact-resistant composite material skateboard, comprising the following steps:
[0033] The high-strength carbon fiber mixed with high modulus carbon fiber two-dimensional braid pre-impregnated with thermosetting resin is embedded in the middle of the stack of aramid fiber or UHMWPE fiber mixed with glass fiber two-dimensional braid pre-impregnated with thermosetting resin, and hot-pressed to form an impact-resistant hybrid fiber composite layer with a high-strength carbon fiber layer set in the core;
[0034] The upper surface friction-resistant layer and the lower surface accessory assembly layer are respectively adhered to the upper and lower surfaces of the impact-resistant mixed fiber composite layer with adhesive, and then subjected to secondary hot pressing molding after drying to obtain the product.
[0035] The present invention does not impose any special restrictions on the hot pressing process of the impact-resistant mixed fiber composite layer with a high-strength carbon fiber layer in the core, and can adopt the commonly used methods in the field. The temperature of the hot pressing is determined according to the selected thermosetting resin, the time of the hot pressing is 10-20 minutes, the pressure is 5-10MPa, and 2-4 exhaust points are set in the middle period of the hot pressing. Finally, the mold is opened and sampled at room temperature after natural cooling.
[0036] The present invention does not impose any special restrictions on the secondary hot pressing process, and the commonly used methods in the art can be used. The adhesive includes but is not limited to any one of epoxy resin adhesive, urea-formaldehyde resin adhesive, phenolic resin adhesive, and melamine-formaldehyde adhesive. The hot pressing time is 5-10 minutes, the pressure is 2-5 MPa, the temperature is 60-150°C, 1-2 exhaust points are set in the middle period of pressing, and finally the mold is opened and sampled at room temperature after natural cooling.
[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0038] Example 1
[0039] This embodiment provides an impact-resistant composite skateboard, and its overall structure schematic diagram is as follows: Figure 1 As shown, from top to bottom, it includes an upper surface friction-resistant layer 3, an impact-resistant hybrid fiber composite layer 2 and a lower surface accessory assembly layer 4; a high-strength carbon fiber layer 1 is arranged at the core of the impact-resistant hybrid fiber composite layer 2; a metal embedded part 5 is arranged on the lower surface accessory assembly layer 4, as shown in FIG. Figure 2 shown.
[0040] The upper surface friction-resistant layer 3 is made of MDI type polyurethane material with a thickness of 0.5 mm.
[0041] The total thickness of the impact-resistant hybrid fiber composite layer 2 is 4 mm, and it covers the high-strength carbon fiber layer 1, which is made of aramid fiber and glass fiber mixed in a mass ratio of 3:1, woven in a two-dimensional twill, and then composited with an unsaturated polyester resin matrix with a resin content of 30%. This layer of two-dimensional woven fabric is processed in a single-layer stacking manner, and the number of layers is 30.
[0042] The thickness of the high-strength carbon fiber layer 1 is 1 mm, and its projection area in the direction parallel to the skateboard surface is 85% of the projection area of the impact-resistant mixed fiber composite layer 2 in the direction parallel to the skateboard surface. This layer is made of T700 high-strength carbon fiber and M55 high-modulus carbon fiber mixed in a mass ratio of 1:1, woven in a two-dimensional twill, and then composited with an epoxy resin matrix with a resin content of 40%. This layer of two-dimensional woven fabric is processed in a single-layer stacking method, with 8 layers of ply.
[0043] The thickness of the lower surface accessory assembly layer 4 is 0.5 mm. It is made of T800 high-strength carbon fiber for two-dimensional plain weaving and then compounded with phenolic resin with a resin content of 40%.
[0044] The T700 high-strength carbon fiber mixed with M55 high-modulus carbon fiber two-dimensional braided fabric pre-impregnated with epoxy resin is embedded in the middle position of the stack of the aramid fiber mixed with glass fiber two-dimensional braided fabric pre-impregnated with unsaturated polyester resin, and hot-pressed at a temperature of 80°C, a time of 10 minutes, and a pressure of 5MPa. Two exhaust points are set in the middle period of hot-pressing, and finally the mold is opened and sampled at room temperature after natural cooling, so as to obtain an impact-resistant hybrid fiber composite layer 2 with a high-strength carbon fiber layer 1 set in the core. The upper surface friction-resistant layer 3 and the lower surface accessory assembly layer 4 are respectively attached to the upper and lower surfaces of the impact-resistant hybrid fiber composite layer 2 with epoxy resin adhesive, and the secondary hot-pressing is performed after natural drying for 15 minutes, at a temperature of 80°C, a time of 5 minutes, and a pressure of 3MPa. One exhaust point is set in the middle period of hot-pressing, and finally the mold is opened and sampled at room temperature after natural cooling, so as to obtain the product.
[0045] Metal embedded parts 5 are installed at front-to-back symmetrical positions on the lower surface accessory assembly layer 4 for connecting the wheel bracket.
[0046] Example 2
[0047] This embodiment provides an impact-resistant composite skateboard, and its overall structure schematic diagram is as follows: Figure 1 As shown, from top to bottom, it includes an upper surface friction-resistant layer 3, an impact-resistant hybrid fiber composite layer 2 and a lower surface accessory assembly layer 4; a high-strength carbon fiber layer 1 is arranged at the core of the impact-resistant hybrid fiber composite layer 2; a metal embedded part 5 is arranged on the lower surface accessory assembly layer 4, as shown in FIG. Figure 2 shown.
[0048] The upper surface friction-resistant layer 3 is made of TDI type polyurethane material with a thickness of 0.3 mm.
[0049] The total thickness of the impact-resistant hybrid fiber composite layer 2 is 6 mm, and it is coated with a high-strength carbon fiber layer 1, which is made of UHMWPE fiber and glass fiber mixed in a mass ratio of 5:1, woven in a two-dimensional plain weave, and then composited with an epoxy resin matrix, with a resin content of 40%. This layer of two-dimensional woven fabric is processed in a single-layer stacking method, with 28 layers of ply.
[0050] The thickness of the high-strength carbon fiber layer 1 is 1.5 mm, and its projection area in the direction parallel to the skateboard surface is 90% of the projection area of the impact-resistant hybrid fiber composite layer 2 in the direction parallel to the skateboard surface. This layer is made of T800 high-strength carbon fiber and M60J high-modulus carbon fiber mixed in a mass ratio of 2:1, woven in a two-dimensional satin weave, and then composited with a urea-formaldehyde resin matrix with a resin content of 50%. The two-dimensional woven fabric is processed in a single-layer stacking method, with 7 layers of ply.
[0051] The thickness of the lower surface accessory assembly layer 4 is 0.5 mm. It is made of T1000 high-strength carbon fiber for two-dimensional twill weaving and then compounded with epoxy resin with a resin content of 30%.
[0052] The T800 high-strength carbon fiber mixed with M60J high-modulus carbon fiber two-dimensional braided fabric pre-impregnated with urea-formaldehyde resin was embedded in the middle position of the stack of the aramid fiber mixed with glass fiber two-dimensional braided fabric pre-impregnated with epoxy resin, and hot-pressed at a temperature of 130°C, a time of 12 minutes, and a pressure of 8MPa. Three exhaust points were set in the middle period of hot-pressing, and finally the mold was opened and sampled at room temperature after natural cooling, and the impact-resistant hybrid fiber composite layer 2 with a high-strength carbon fiber layer 1 in the core was obtained. The upper surface friction-resistant layer 3 and the lower surface accessory assembly layer 4 were respectively attached to the upper and lower surfaces of the impact-resistant hybrid fiber composite layer 2 with epoxy resin adhesive, and the secondary hot-pressing was performed after natural drying for 15 minutes, at a temperature of 80°C, a time of 5 minutes, and a pressure of 3MPa. One exhaust point was set in the middle period of hot-pressing, and finally the mold was opened and sampled at room temperature after natural cooling, and the result was obtained.
[0053] Metal embedded parts 5 are installed at front-to-back symmetrical positions on the lower surface accessory assembly layer 4 for connecting the wheel bracket.
[0054] Example 3
[0055] This embodiment provides an impact-resistant composite skateboard, and its overall structure schematic diagram is as follows: Figure 1 As shown, from top to bottom, it includes an upper surface friction-resistant layer 3, an impact-resistant hybrid fiber composite layer 2 and a lower surface accessory assembly layer 4; a high-strength carbon fiber layer 1 is arranged at the core of the impact-resistant hybrid fiber composite layer 2; a metal embedded part 5 is arranged on the lower surface accessory assembly layer 4, as shown in FIG. Figure 2 shown.
[0056] The upper surface friction-resistant layer 3 is made of TDI type polyurethane material with a thickness of 0.6 mm.
[0057] The total thickness of the impact-resistant hybrid fiber composite layer 2 is 7 mm, and it covers the high-strength carbon fiber layer 1, which is made of UHMWPE fiber and glass fiber mixed in a mass ratio of 7:1, woven in a two-dimensional plain weave, and then composited with a phenolic resin matrix, with a resin content of 40%. This layer of two-dimensional woven fabric is processed in a single-layer stacking manner, with 30 layers of ply.
[0058] The thickness of the high-strength carbon fiber layer 1 is 2 mm, and its projection area in the direction parallel to the skateboard surface is 95% of the projection area of the impact-resistant mixed fiber composite layer 2 in the direction parallel to the skateboard surface. This layer is made of T300 high-strength carbon fiber and M55J high-modulus carbon fiber mixed in a mass ratio of 3:1, woven in a two-dimensional plain weave, and then composited with a urea-formaldehyde resin matrix with a resin content of 40%. This layer of two-dimensional woven fabric is processed in a single-layer stacking method, with 9 layers of ply.
[0059] The thickness of the lower surface accessory assembly layer 4 is 0.8 mm. It is made of T800 high-strength carbon fiber for two-dimensional twill weaving and then compounded with epoxy resin with a resin content of 30%.
[0060] The T300 high-strength carbon fiber mixed with M55J high-modulus carbon fiber two-dimensional braided fabric pre-impregnated with urea-formaldehyde resin was embedded in the middle position of the stack of the aramid fiber mixed with glass fiber two-dimensional braided fabric pre-impregnated with phenolic resin, and hot-pressed at a temperature of 140°C, a time of 12 minutes, and a pressure of 8MPa. Three exhaust points were set in the middle period of hot-pressing, and finally the mold was opened and sampled at room temperature after natural cooling, and the impact-resistant hybrid fiber composite layer 2 with a high-strength carbon fiber layer 1 in the core was obtained. The upper surface friction-resistant layer 3 and the lower surface accessory assembly layer 4 were respectively attached to the upper and lower surfaces of the impact-resistant hybrid fiber composite layer 2 with phenolic resin adhesive, and the secondary hot-pressing was performed after natural drying for 20 minutes, at a temperature of 130°C, a time of 10 minutes, and a pressure of 5MPa. One exhaust point was set in the middle period of hot-pressing, and finally the mold was opened and sampled at room temperature after natural cooling, and the result was obtained.
[0061] Metal embedded parts 5 are installed at front-to-back symmetrical positions on the lower surface accessory assembly layer 4 for connecting the wheel bracket.
[0062] Example 4
[0063] This embodiment provides an impact-resistant composite skateboard, and its overall structure schematic diagram is as follows: Figure 1 As shown, from top to bottom, it includes an upper surface friction-resistant layer 3, an impact-resistant hybrid fiber composite layer 2 and a lower surface accessory assembly layer 4; a high-strength carbon fiber layer 1 is arranged at the core of the impact-resistant hybrid fiber composite layer 2; a metal embedded part 5 is arranged on the lower surface accessory assembly layer 4, as shown in FIG. Figure 2 shown.
[0064] The upper surface friction-resistant layer 3 is made of NDI type polyurethane material with a thickness of 0.3 mm.
[0065] The total thickness of the impact-resistant hybrid fiber composite layer 2 is 8 mm, and it covers the high-strength carbon fiber layer 1, which is made of UHMWPE fiber and glass fiber mixed in a mass ratio of 5:1, woven in a two-dimensional plain weave, and then composited with an epoxy resin matrix, with a resin content of 50%. This layer of two-dimensional woven fabric is processed in a single-layer stacking method, with 40 layers of ply.
[0066] The thickness of the high-strength carbon fiber layer 1 is 2 mm, and its projection area in the direction parallel to the skateboard surface is 80% of the projection area of the impact-resistant mixed fiber composite layer 2 in the direction parallel to the skateboard surface. This layer is made of T800 high-strength carbon fiber and M40 high-modulus carbon fiber mixed in a mass ratio of 1:1, woven in a two-dimensional twill, and then composited with a urea-formaldehyde resin matrix with a resin content of 50%. This layer of two-dimensional woven fabric is processed in a single-layer stacking method, with 12 layers of ply.
[0067] The thickness of the lower surface accessory assembly layer 4 is 0.7 mm. It is made of T1000 high-strength carbon fiber for two-dimensional twill weaving and then compounded with epoxy resin with a resin content of 30%.
[0068] The T700 high-strength carbon fiber mixed with M55 high-modulus carbon fiber two-dimensional braided fabric pre-impregnated with epoxy resin is embedded in the middle position of the stack of the aramid fiber mixed with glass fiber two-dimensional braided fabric pre-impregnated with urea-formaldehyde resin, and hot-pressed at a temperature of 130°C, a time of 15 minutes, and a pressure of 10MPa. Three exhaust points are set in the middle period of hot-pressing, and finally the mold is opened and sampled at room temperature after natural cooling, so as to obtain an impact-resistant hybrid fiber composite layer 2 with a high-strength carbon fiber layer 1 set in the core. The upper surface friction-resistant layer 3 and the lower surface accessory assembly layer 4 are respectively attached to the upper and lower surfaces of the impact-resistant hybrid fiber composite layer 2 with urea-formaldehyde resin adhesive, and the secondary hot-pressing is performed after natural drying for 20 minutes, at a temperature of 130°C, a time of 8 minutes, and a pressure of 5MPa. Two exhaust points are set in the middle period of hot-pressing, and finally the mold is opened and sampled at room temperature after natural cooling, so as to obtain the product.
[0069] Metal embedded parts 5 are installed at front-to-back symmetrical positions on the lower surface accessory assembly layer 4 for connecting the wheel bracket.
[0070] Test example
[0071] The performance of the impact-resistant composite skateboards of Examples 1 to 4 was measured, wherein the shear strength was tested with reference to GB / T20241-2006 "Laminated Veneer Timber", the flexural strength was tested with reference to GB / T 3356-2014 "Test Method for Flexural Properties of Oriented Fiber Reinforced Polymer Matrix Composite Materials", the tensile strength was tested with reference to GB / T1040-2006 "Test Method for Tensile Properties of Plastics", and the impact toughness was tested with reference to the three-point bending impact test scheme in ASTM D143-2014. The test results are shown in Table 1. It can be seen that the impact-resistant composite skateboard provided in the embodiment has a performance improvement of about 30-50% relative to the commercially available seven-layer maple sports skateboard, and has good comprehensive mechanical properties.
[0072] Table 1 Test results of the impact-resistant composite skateboard performance of Examples 1 to 4
[0073]
[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An impact-resistant composite skateboard, characterized in that: The upper surface friction-resistant layer, the impact-resistant hybrid fiber composite layer and the lower surface accessory assembly layer are sequentially included from top to bottom; the core of the impact-resistant hybrid fiber composite layer is provided with a high-strength carbon fiber layer; the projection area of the high-strength carbon fiber layer in the direction parallel to the surface of the impact-resistant composite skateboard accounts for 80-95% of the projection area of the impact-resistant hybrid fiber composite layer in the direction parallel to the surface of the impact-resistant composite skateboard; The upper surface friction-resistant layer is a polyurethane layer; the impact-resistant hybrid fiber composite layer is made of aramid fiber or UHMWPE fiber mixed with glass fiber two-dimensional braided fabric reinforced with thermosetting resin; The lower surface accessory assembly layer is made of high-strength carbon fiber two-dimensional braided fabric reinforced with thermosetting resin, and a metal embedded part is arranged on the lower surface accessory assembly layer; the high-strength carbon fiber layer is made of high-strength carbon fiber mixed with high-modulus carbon fiber two-dimensional braided fabric reinforced with thermosetting resin; The method for preparing the impact-resistant composite material skateboard comprises the following steps: The high-strength carbon fiber mixed with high modulus carbon fiber two-dimensional braid pre-impregnated with thermosetting resin is embedded in the middle of the stack of aramid fiber or UHMWPE fiber mixed with glass fiber two-dimensional braid pre-impregnated with thermosetting resin, and hot-pressed to form an impact-resistant hybrid fiber composite layer with a high-strength carbon fiber layer set in the core; The upper surface friction-resistant layer and the lower surface accessory assembly layer are respectively pasted on the upper and lower surfaces of the impact-resistant mixed fiber composite layer, and then subjected to secondary hot pressing molding after drying to obtain the product.
2. The impact-resistant composite skateboard according to claim 1, characterized in that: The polyurethane material of the polyurethane layer is selected from any one of an MDI type polyurethane material, a TDI type polyurethane material or an NDI type polyurethane material.
3. The impact-resistant composite skateboard according to claim 1, characterized in that: The mixed mass ratio of the aramid fiber or UHMWPE fiber to the glass fiber is (2-10):
1.
4. The impact-resistant composite skateboard according to claim 1, characterized in that: The structures of the two-dimensional braids of the impact-resistant hybrid fiber composite layer, the lower surface accessory assembly layer and the high-strength carbon fiber layer are independently selected from any one of plain, twill or satin weaving structures.
5. The impact-resistant composite skateboard according to claim 1, characterized in that: The thermosetting resins of the impact-resistant hybrid fiber composite layer, the lower surface accessory assembly layer and the high-strength carbon fiber layer are independently selected from any one of epoxy resin, phenolic resin, unsaturated polyester resin or urea-formaldehyde resin, and the resin content is 30-60wt%.
6. The impact-resistant composite skateboard according to claim 1, characterized in that: The high-strength carbon fibers of the lower surface accessory assembly layer and the high-strength carbon fiber layer are each independently selected from any one of T300, T700, T800 or T1000.
7. The impact-resistant composite skateboard according to claim 1, characterized in that: The mixed mass ratio of the high-strength carbon fiber and the high modulus carbon fiber in the high-strength carbon fiber layer is (1-3):1; the high modulus carbon fiber in the high-strength carbon fiber layer is selected from any one of M40, M55, M60, M40J, M55J or M60J.
8. The impact-resistant composite skateboard according to claim 1, characterized in that: The thickness of the friction-resistant layer on the upper surface is 0.2-1 mm, the thickness of the impact-resistant mixed fiber composite layer is 3-8 mm, the thickness of the lower surface accessory assembly layer is 0.5-1 mm; and the thickness of the high-strength carbon fiber layer is 1-3 mm.
9. The method for preparing the impact-resistant composite material skateboard according to any one of claims 1 to 8, characterized in that: The steps include: The high-strength carbon fiber mixed with high modulus carbon fiber two-dimensional braid pre-impregnated with thermosetting resin is embedded in the middle of the stack of aramid fiber or UHMWPE fiber mixed with glass fiber two-dimensional braid pre-impregnated with thermosetting resin, and hot-pressed to form an impact-resistant hybrid fiber composite layer with a high-strength carbon fiber layer set in the core; The upper surface friction-resistant layer and the lower surface accessory assembly layer are respectively pasted on the upper and lower surfaces of the impact-resistant mixed fiber composite layer, and then subjected to secondary hot pressing molding after drying to obtain the product.