A method for improving the spheroidization rate of copper smelting prills

By mixing bentonite and quartz sand to form primary sand during the copper smelting granulation process, and then mixing it with copper concentrate and coal, followed by spray hydration granulation, the problem of low particle formation rate in copper smelting granulation was solved, achieving efficient waste heat recovery and clean production.

CN118127319BActive Publication Date: 2026-11-20YUNNAN COPPER CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410015215.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-04
Publication Date
2026-11-20
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

The low pelletizing rate in copper smelting and granulation results in a large amount of powdery material that does not form particles, leading to a decrease in waste heat recovery rate, an increase in metal loss, and pollution of the site environment.

Method used

In the copper smelting granulation process, bentonite and quartz sand are mixed to form primary sand, which is then mixed with copper concentrate and coal and fed into a granulator. Water is sprayed to granulate the particles, and the moisture content of the particles is adjusted to improve the pelletizing rate.

Benefits of technology

It increases the pelletizing rate of copper smelting particles by more than 20%, reduces the amount of unpelleted powdery material, reduces material flying, improves waste heat recovery efficiency, reduces dust rate, increases direct metal recovery rate, and achieves clean production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118127319B_ABST
    Figure CN118127319B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of metal smelting, and particularly relates to a method for improving the pelletizing rate of copper smelting granules, comprising the following steps: mixing bentonite and quartz sand to obtain primary sand; mixing mixed copper concentrate, coal and the primary sand to obtain a mixture; feeding the mixture into a pelletizer and spraying water to pelletize the mixture to obtain granules, thereby improving the pelletizing rate of copper smelting granules. By using the ratio of bentonite to mixed copper concentrate, the water content of the granules is adjusted, the pelletizing rate of copper smelting is increased by more than 20%, the amount of un-pelletized powdery material is reduced, and the material flying in the transportation process is avoided. The method can effectively reduce the remaining powdery material after pelletizing, effectively reduce the copper-containing material drawn into the flue of the waste heat boiler, improve the waste heat recovery efficiency, reduce the copper smelting dust rate, reduce the dust collection process pressure, improve the metal direct recovery rate, ensure the orderly and efficient production organization of the smelting furnace, and realize clean production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal smelting technology, and in particular to a method for improving the pelletizing rate of copper smelting particles. Background Technology

[0002] In the process of preparing raw materials for copper smelting, powdered materials such as copper concentrate, flux, and coal with a certain moisture content are fed into a rotating granulator through a conveying system. Water is sprayed from above the granulator, and the material and water droplets combine to form mother balls. The mother balls roll in the granulator, and the surface of the mother balls is continuously coated with powdered material to form particles of a certain diameter. The particles and the powdered material that has not formed particles fall into the smelting furnace through the feed port via the granulator and conveying system.

[0003] However, existing copper smelting granulation particle preparation processes have the following problems:

[0004] 1. The particle spheroidization rate is low, and the amount of powdery material that does not form particles is large;

[0005] 2. During transportation, due to the different horizontal heights of the various belt conveyors, there is a drop, and powdery materials that have not formed particles fly at the discharge ports of each belt, causing metal loss and polluting the on-site working environment.

[0006] 3. Powdered materials that have not yet formed particles enter the relatively large furnace through the feed port. Due to the negative pressure inside the furnace, the material enters the waste heat boiler flue as mechanical dust, adhering to the inner wall of the waste heat boiler flue, the horizontal flue tube screen and bundle, and the horizontal flue pipes, causing a series of serious copper smelting problems. The main problems are: Mechanical dust adhering to the waste heat boiler cooling water pipes reduces the flue gas heat exchange effect, lowering waste heat recovery efficiency; it also reduces the volume of the waste heat boiler flue, obstructing flue gas flow, causing flue gas to escape from the furnace top, polluting the on-site working environment. Smelting furnaces typically reduce production load, significantly impacting copper concentrate processing capacity; mechanical dust entering the subsequent flue gas treatment system increases the difficulty and cost of subsequent flue gas treatment, leading to the loss of copper-containing materials and increased metal loss.

[0007] Therefore, existing technologies still need to be improved and developed. Summary of the Invention

[0008] In view of the shortcomings of the prior art, the purpose of this invention is to provide a method for improving the pelletizing rate of copper smelting granules, aiming to solve the problems of low pelletizing rate of existing copper smelting granules and reduced waste heat recovery rate caused by powdery materials that do not form particles.

[0009] The technical solution of the present invention is as follows:

[0010] A method for improving the pelletizing rate of copper smelting particles includes the following steps:

[0011] Bentonite and quartz sand are mixed to obtain primary sand;

[0012] The mixed copper concentrate, coal, and primary sand are mixed to obtain a mixture;

[0013] The mixture is fed into a granulator and granulated by spraying water to obtain particles, thereby improving the pelletizing rate of copper smelting granules.

[0014] The method for improving the pelletizing rate of copper smelting granulation particles, wherein the mass ratio of bentonite to quartz sand is 1:7-3:7.

[0015] The method for improving the pelletizing rate of copper smelting granulation particles, wherein the mass of the primary sand accounts for 4%-10% of the mass of the mixed copper concentrate.

[0016] The method for improving the pelletizing rate of copper smelting granulation particles, wherein the water content of the mixed copper concentrate is 7.5%-8.5%.

[0017] The method for improving the pelletizing rate of copper smelting granulation particles, wherein the mass ratio of the coal to the mixed copper concentrate is 1%-4%.

[0018] The method for improving the pelletizing rate of copper smelting granulation particles includes a pellet mill with a diameter of 4.5m-5.5m, a disc tilt angle of 35°-50°, and a maximum disc rotation speed of 8r / min.

[0019] The method for improving the pelletizing rate of copper smelting granules, wherein the moisture content of the particles is 13%-15%.

[0020] The method for improving the pelletizing rate of copper smelting granulation particles, wherein the particle size is 6mm-39mm.

[0021] Beneficial Effects: This invention provides a method for improving the pelletizing rate of copper smelting particles, comprising the steps of: mixing bentonite and quartz sand to obtain primary sand; mixing mixed copper concentrate, coal, and the primary sand to obtain a mixture; feeding the mixture into a pelletizer and granulating it by spraying water to obtain particles, thereby improving the pelletizing rate of copper smelting particles. This invention, by utilizing the ratio of bentonite to mixed copper concentrate and adjusting particle moisture control, increases the pelletizing rate of copper smelting particles by more than 20%, reduces the amount of ungranulated powdery material, and avoids material scattering during transportation. The method for improving the pelletizing rate of copper smelting particles provided by this invention can effectively reduce the residual powdery material after granulation, effectively reduce the amount of copper-containing material drawn into the waste heat boiler flue, improve waste heat recovery efficiency, reduce copper smelting dust rate, reduce the pressure of the dust collection process, increase the direct metal recovery rate, ensure orderly and efficient production organization of the smelting furnace, and achieve clean production. Attached Figure Description

[0022] Figure 1 This is a schematic flowchart of a method for improving the pelletizing rate of copper smelting particles according to the present invention. Detailed Implementation

[0023] This invention provides a method for improving the pelletizing rate of copper smelting particles. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0024] It will be understood by those skilled in the art that, unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. It should also be understood that terms such as those defined in general dictionaries should be understood to have the same meaning as in the context of the prior art, and should not be interpreted in an idealized or overly formal sense unless specifically defined as herein.

[0025] The basic principle of granulation: When a mixture of coal, flux, and copper concentrate is wetted by water, the particles around the water droplet are pulled toward the center of the droplet by capillary force to form a mother ball. In the granulator, with the help of rolling and rubbing, a layer of powdery material adheres to the surface of the mother ball, causing the mother ball to grow and become compact, producing granules.

[0026] However, existing copper smelting granulation particle preparation processes suffer from problems such as low pelletizing rate and reduced waste heat recovery rate due to powdery materials that do not form particles.

[0027] Based on this, such as Figure 1 As shown, the present invention provides a method for improving the pelletizing rate of copper smelting particles, comprising the following steps:

[0028] Step S10: Mix bentonite with quartz sand to obtain primary sand;

[0029] Step S20: Mix the mixed copper concentrate, coal and the primary sand to obtain a mixture;

[0030] Step S30: The mixture is fed into a granulator and granulated by spraying water to improve the pelletizing rate of copper smelting particles.

[0031] In this embodiment, bentonite and quartz sand are first mixed to obtain primary sand, which is then mixed with mixed copper concentrate and coal for granulation, thereby improving the pelletizing rate of copper smelting particles. The bentonite disperses into monomers upon contact with water, filling the voids in the mixed copper concentrate powder particles. These monomers have strong colloidal properties, enhancing the bonding of the mineral powder. Simultaneously, due to their strong adsorption capacity, they can form an adsorbed water layer on the surface of the green pellets. This allows the particles within the pellets to slide against each other when impacted, resulting in plastic deformation and preventing breakage, thus improving the pelletizing rate of copper smelting particles. Furthermore, by utilizing the ratio of bentonite to mixed copper concentrate and adjusting particle moisture control, this invention increases the granulation rate of copper smelting by more than 20%, reduces the amount of ungranulated powdery material, avoids material flying during transportation, effectively reduces the amount of material being drawn into the waste heat boiler flue after entering the furnace, improves waste heat recovery efficiency, reduces the copper smelting dust rate by about 0.2%, reduces the pressure of the dust collection process, increases the direct metal recovery rate, ensures orderly and efficient production organization of the smelting furnace, and achieves clean production.

[0032] Specifically, the use of bentonite in the copper smelting granulation process can increase the pelletizing rate of copper smelting particles by more than 20% and reduce the amount of ungranulated powdery material. Bentonite reagent has strong hygroscopic and swelling properties, capable of absorbing 8-15 times its own volume of water, with a volume expansion of several to 30 times. In aqueous media, it can disperse into gel-like and suspension states. This solution exhibits certain viscosity, thixotropy, and lubricity, and possesses strong cation exchange capacity. Furthermore, bentonite is effective against various gases, liquids, and organic substances. It has a certain adsorption capacity, with a maximum adsorption capacity of up to 5 times its own weight. Its mixture with water, mud, or fine sand has plasticity and cohesiveness. When bentonite comes into contact with water, it quickly disperses into monomers with several crystalline layers, filling the gaps between concentrate powder particles. Due to the strong colloidal properties of these monomers, they can enhance the bonding effect of the mineral powder. In addition, due to its strong adsorption effect, it can form an adsorbed water layer on the surface of green pellets, which allows the particles in the pellets to slide against each other when the green pellets are impacted, thereby producing plastic deformation and preventing them from breaking.

[0033] Bentonite is a non-metallic mineral with montmorillonite as its main mineral component. Montmorillonite has a 2:1 crystal structure consisting of two silicon-oxygen tetrahedra sandwiching a layer of aluminum-oxygen octahedra. Due to the presence of certain cations such as Cu, Mg, Na, and K in the layered structure formed by the montmorillonite unit cells, and the fact that these cations are unstable with the montmorillonite unit cells and easily exchanged with other cations, it exhibits good ion exchange properties. The type of interlayer cation in bentonite determines its type; the interlayer cation is Na. + It is called sodium-based bentonite; the interlayer cation is Ca. 2+ It was then called calcium-based bentonite; the interlayer cation was H. + It is sometimes called hydrogen-based bentonite (activated clay, natural bleaching clay - acidic clay); when the interlayer cations are organic cations, it is called organic bentonite. Bentonite has strong hygroscopicity and swelling properties, capable of adsorbing 8 to 15 times its own volume of water, with a volume expansion of several to 30 times. In aqueous media, it can disperse into gel-like and suspension states, and this medium solution has certain viscosity, thixotropy, and lubricity. It has a strong cation exchange capacity; it has a certain adsorption capacity for various gases, liquids, and organic substances, with a maximum adsorption capacity of up to 5 times its own weight; its mixture with water, mud, or fine sand has plasticity and binding properties; surface-active acidic bleaching clay (activated clay, natural bleaching clay - acidic clay) can adsorb colored ions.

[0034] In some embodiments, the mass ratio of bentonite to quartz sand is 1:7 to 3:7. Mixing bentonite and quartz sand in this ratio and using it as primary sand can improve the pelletizing rate of copper smelting granules without wasting bentonite reagent.

[0035] Specifically, bentonite and quartz sand are mixed in the open air, rather than being added to the pellet mill as a separate material via a concentrate silo, feed disc, and conveyor belt. The advantages of doing so are: first, it eliminates the impact of seepage and water accumulation in the concentrate silo on the bentonite; second, it avoids low-altitude pollution during the process of unloading the concentrate from the concentrate silo to the feed silo by the crane; third, it avoids the stratification of bentonite and concentrate on the conveyor belt; and fourth, it avoids measurement errors of the belt scale.

[0036] In a preferred embodiment, the mass ratio of the bentonite to the quartz sand is 1:3.

[0037] In some embodiments, the mass of the primary sand accounts for 4%-10% of the mass of the mixed copper concentrate.

[0038] Specifically, the amount of primary sand added is determined according to the requirements of the smelting slag type; preferably, the mass of the primary sand accounts for 4% of the mass of the mixed copper concentrate.

[0039] In some embodiments, the moisture content of the mixed copper concentrate is 7.5%-8.5%. Controlling the moisture content of the raw material mixed copper concentrate between 7.5% and 8.5% during the preparation of copper smelting granules can prevent the mixed copper concentrate from flying during transportation into the granulator and also lay the foundation for moisture requirements in the control of granulated particles.

[0040] In a preferred embodiment, the moisture content of the mixed copper concentrate is 8%-8.5%, which is intended to prevent the mixed copper concentrate from flying away during transportation into the granulator and to lay the foundation for moisture requirements for controlling the granulated particles.

[0041] In some embodiments, the mass ratio of the coal to the mixed copper concentrate is 1%-4%, which is the normal range for the embodiments and does not include special cases; this mass ratio is mainly determined by the copper smelting process.

[0042] In some embodiments, the granulator has a diameter of 4.5m-5.5m, a disc tilt angle of 35°-50°, and a maximum disc rotation speed of 8r / min.

[0043] In a preferred embodiment, the pellet mill has a diameter of 5.5m, a disc tilt angle of 35°-50°, and a maximum disc rotation speed of 7.97r / min, thereby improving pelleting efficiency.

[0044] Specifically, there are 5 pellet mills, each with a diameter of 5.5m and a maximum disc rotation speed of 7.97r / min. The disc tilt angle can be adjusted according to the material feed rate of each pellet mill and the material adhesion characteristics to obtain the best pelleting effect. In this embodiment, the disc tilt angle is 35-45°.

[0045] In some embodiments, the moisture content of the particles is 13%-15%. Controlling the moisture content of the final particles to 13%-15% satisfies the strong hygroscopicity of bentonite, thereby improving the particle pelleting rate. If the moisture content is below 13%, the result will be the opposite, leading to a worse pelleting rate.

[0046] In this embodiment, each granulator is equipped with an atomizing nozzle, which is connected by a water pipe and a compressed air pipe, each with a valve. The opening of the water pipe and compressed air pipe valves can be adjusted according to the feed rate of a single hopper and the pelleting situation to obtain the best atomization effect and ensure that the particle moisture content is controlled at 13-15%. Because the reagent has strong hygroscopic properties, the particle moisture content needs to be increased by 2-3% without adding the reagent to achieve good results. If the moisture content is not increased accordingly, the result will be counterproductive.

[0047] In some embodiments, the particle size is 6-39 mm.

[0048] In some embodiments, the method for calculating the pelletizing rate of copper smelting granulation particles is as follows: the downstream conveyor belt of the granulator is used as the sampling point, the sampling frequency is once every 2 hours, the shovel is used as the sampling tool, the sample is screened, and the particles are weighed before and after screening. Under normal circumstances, the particles are considered to be of the same size (i.e., the weight is consistent), and the mass percentage is used as the pelletizing rate.

[0049] Specifically, the steps for calculating the pelletizing rate of the copper smelting granulation particles include:

[0050] 1. Sampling: When sampling, it is required to use a shovel to dig all the way to the bottom;

[0051] 2. Sorting: Sorting out and discarding particles with a diameter ≥40mm from the sample;

[0052] 3. Weighing: Weigh the sorted samples for the first time and record the total weight m;

[0053] 4. Sieving: Use a sieve to remove powdery materials from the sample; the remaining material is qualified particles.

[0054] 5. Secondary weighing: Weigh the qualified particles and record the weight m1;

[0055] 6. Calculation: Ball formation rate = m1 ÷ m × 100%.

[0056] The following examples further illustrate the present invention in detail. It should also be understood that the following examples are only for further explanation of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention are within the scope of protection of the present invention.

[0057] Example 1

[0058] This embodiment provides a process for granulating copper concentrate, including the following steps:

[0059] By mass percentage, 1 wt% bentonite and 3 wt% quartz sand are mixed to obtain primary sand; mixed copper concentrate with a moisture content of 8%-8.5% and 2.5% coal and primary sand are mixed to obtain a mixture; the mixture is fed into a granulator, and water is sprayed from above the granulator. The amount of water sprayed is adjusted to meet the moisture requirements of bentonite, and the moisture content of the resulting particles is controlled to be 13%. The particles and the powdery material that has not formed particles fall into the smelting furnace through the feed port after passing through the granulator and the conveying system.

[0060] Examples 2-4 (Note: For ease of comparison with Comparative Example 1, the amount of bentonite is not included in the quartz sand in Table 1)

[0061] The difference from Example 1 is that the amount of bentonite and quartz sand added is different, as is the moisture content of the particles, as shown in Table 1.

[0062] Comparative Example 1

[0063] The difference from Example 1 is that the amount of bentonite and quartz sand added is different, as is the moisture content of the particles, as shown in Table 1.

[0064] The ball formation rate of Examples 1-4 and Comparative Example 1 was calculated, and the ball formation rate data are shown in Table 1.

[0065]

[0066] When quartz sand accounts for 3-7% of the mixed copper concentrate, 1-3% bentonite is added, the moisture content of the granulated particles is controlled at 13-14%, and the pelletizing rate of the granulated particles reaches more than 90%, which is more than 20% higher than the pelletizing rate when no bentonite is added.

[0067] In summary, this invention provides a method for improving the pelletizing rate of copper smelting particles, comprising the steps of: mixing bentonite and quartz sand to obtain primary sand; mixing mixed copper concentrate, coal, and the primary sand to obtain a mixture; feeding the mixture into a pelletizer and granulating it by spraying water to obtain particles, thereby improving the pelletizing rate of copper smelting particles. This invention, by utilizing the ratio of bentonite to mixed copper concentrate and adjusting particle moisture control, increases the pelletizing rate of copper smelting particles by more than 20%, reduces the amount of unparticled powdery material, and avoids material scattering during transportation. The method for improving the pelletizing rate of copper smelting particles provided by this invention can effectively reduce the residual powdery material after granulation, effectively reduce the amount of copper-containing material drawn into the waste heat boiler flue, improve waste heat recovery efficiency, reduce copper smelting dust rate, reduce the pressure of the dust collection process, increase the direct metal recovery rate, ensure orderly and efficient production organization of the smelting furnace, and achieve clean production.

[0068] It should be understood that the application of the present invention is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A method for improving the pelletizing rate of copper smelting particles, characterized in that, Including the following steps: Bentonite and quartz sand are mixed to obtain primary sand; The mixed copper concentrate, coal, and primary sand are mixed to obtain a mixture; The mixture is fed into a granulator and granulated by spraying water to obtain particles, thereby improving the pelletizing rate of copper smelting granules. The mass ratio of bentonite to quartz sand is 1:3; the mass of primary sand accounts for 4% of the mass of the mixed copper concentrate; the moisture content of the mixed copper concentrate is 8%-8.5%. The mass ratio of the coal to the mixed copper concentrate is 1%-4%; the moisture content of the particles is 13%-15%; and the particle size is 6mm-39mm.

2. The method for improving the pelletizing rate of copper smelting particles according to claim 1, characterized in that, The granulator has a diameter of 4.5m-5.5m, a disc tilt angle of 35°-50°, and a maximum disc rotation speed of 8r / min.

Citation Information

Patent Citations

  • Method for combined treatment of copper slags and steel slags

    CN105861845A

  • Production method of silicon-chromium alloy

    CN107699685A