Aluminum and titanium controlled oxygen-free protective atmosphere electroslag remelting method
By using a multifunctional protective atmosphere vacuum pressurized electroslag furnace and low residual oxide refining slag in the electroslag remelting process, combined with high-purity argon and electromagnetic stirring, the problem of poor sealing effect of the protective atmosphere electroslag furnace was solved, and low burn-off and compositional uniformity of Al and Ti steel grades were achieved.
Patent Information
- Application Number
- CN202410243685.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-04
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-04
AI Technical Summary
In the existing technology, the sealing effect of the protective atmosphere electroslag furnace is not good, which makes it impossible to reduce the oxygen content in the furnace to 0 ppm, affecting the production of Al and Ti steels, resulting in severe burning loss of Al and Ti elements, as well as increased inclusions and uneven composition.
A multifunctional protective atmosphere vacuum pressurized electroslag furnace is adopted, combining refined slag with low residual oxides and high-purity argon gas. Electromagnetic stirring is achieved through coaxial conductivity, controlling the oxygen content in the furnace to 0 ppm, avoiding the addition of deoxidizers. The refined slag composition is CaF₂: 65-70%, Al₂O₃: 25-30%, MgO: 2-5%, SiO₂≤0.01%, FeO≤0.003%, H₂O≤0.5%. Voltage and current are controlled during electroslag remelting to achieve uniform steel composition.
It effectively reduced the burn-off of Al and Ti to within 8%, stably controlled the deviation of Al and Ti content in the upper and lower parts of the electroslag ingot to ≤5%, ensured the uniformity of Al and Ti content in the electroslag ingot, and avoided the increase of inclusions.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electroslag remelting technology, specifically relating to a method for electroslag remelting in an oxygen-free protective atmosphere with controlled aluminum and titanium. Background Technology
[0002] Currently, domestic protective atmosphere electroslag remelting furnaces use a method of directly adding a fume hood to the crystallizer, which has poor sealing performance and cannot reduce the oxygen content in the furnace to 0 ppm for electroslag remelting. Panzhihua Changgang's 18t protective atmosphere furnace can only control the oxygen content in the furnace below 2000 ppm for arc initiation and slag formation before starting electroslag remelting, while Panzhihua Iron and Steel Research Institute's 150kg protective atmosphere electroslag remelting furnace can only control the oxygen content in the furnace below 200 ppm for arc initiation and slag formation before starting electroslag remelting. Smelting under oxygen conditions is unfavorable for the production of steels containing Al and Ti, as oxygen in the furnace will pass through the furnace chamber-slag-steel mixture, causing easily oxidized elements Al and Ti in the steel to burn off.
[0003] Currently, domestic electroslag ingot manufacturers generally use pre-melted slag to produce Al and Ti-containing steel grades. This pre-melted slag is usually added directly during production, and inevitably, a certain amount of H2O is present in the slag. During the slag-forming period, oxygen is released into the molten steel, reacting with the Al and Ti in the Al and Ti-containing steel, causing Al and Ti to burn off. The total oxide inclusions in domestically produced pre-melted slag are relatively high, ranging from 0.8% to 2%. The total oxide inclusions in electroslag slag produced by Wacker Chemie AG in Germany are 0.8% to 1%, with a few reaching 0.7%, indicating inconsistent quality. Oxide inclusions such as FeO and SiO2 also enter the molten steel, reacting with the Al and Ti in the Al and Ti-containing steel, causing Al and Ti to burn off. Especially when SiO2 is present in the slag, the Al and Ti in the steel will directly reduce Si in the slag into the steel. Easily oxidizable elements such as Al and Ti will enter the slag in the form of oxides, further increasing the burn-off of easily oxidizable Al and Ti in the steel.
[0004] Currently, the Al content loss after electroslag remelting (ESR) of Al and Ti-containing steel ingots under a protective atmosphere exceeds 20%, with significant differences in Al content between the upper and lower parts of the ingot. The only way to reduce the loss of easily oxidized Al and Ti elements is to add deoxidizers such as Al powder or Ca-Si powder during ESR remelting under a protective atmosphere. While this smelting method reduces the loss of easily oxidized Al and Ti elements, it increases the inclusion content of the steel. Practice shows that adding approximately 150 g / t of Al deoxidizer per ton of steel increases the fineness (D) of the ESR ingot by 0.5; adding 150 g / t of Ca-Si powder does not have the same deoxidizing effect as Al deoxidizer, and the increase in inclusions in the ESR ingot is even greater. Summary of the Invention
[0005] To overcome the shortcomings of the existing technology, this invention controls the O content in the electroslag remelting furnace to 0 ppm and uses slag with low residual oxides. This reduces the Al and Ti loss in Al- and Ti-containing electroslag ingots, controlling the loss to within 8%. It also stably controls the deviation of Al and Ti content between the upper and lower parts of the electroslag ingot to ≤5%, ensuring the uniformity of Al and Ti content in the ingot. Because no deoxidizer is added, it does not increase or decrease the formation of inclusions in the steel.
[0006] To achieve the above-mentioned objectives, this invention provides a method for controlled aluminum and titanium electroslag remelting under an oxygen-free protective atmosphere, the method comprising the following technical solutions:
[0007] ① It is produced using a multi-functional protective atmosphere vacuum pressure electroslag furnace, and the consumable electrodes and slag are pretreated.
[0008] ② The basic electrical system for electroslag remelting is a voltage of 20-50V and a current of 700-4500A; an appropriate amount of conductive slag containing TiO2 is added to initiate the arc according to the composition of the smelting steel; the ingot ignition plate is made of the same steel as the electroslag ingot, and rust is removed by shot blasting or laser rust removal machine.
[0009] ③ When the electroslag remelting smelting begins, high-purity argon gas is first introduced, and the oxygen detection equipment is turned on to reduce the oxygen in the furnace to 0 ppm; after the oxygen in the furnace is reduced to 0 ppm, the arc ignition and slag formation are started, and the voltage is controlled at 20-46V and the current is controlled at 700-2900A.
[0010] ④ After slag formation is completed, the oxygen level in the furnace will drop to 0 ppm again (during slag formation, the slag material and consumable electrodes will produce decomposed oxygen), and then electroslag refining will begin. During the electroslag refining period, the voltage will be controlled at 30-32V and the current at 2400-2750A. During the feeding period, the time will be controlled within 5 minutes, the voltage will remain unchanged, and the current will decrease by 500-700A per minute.
[0011] ⑤ Power off and cool in mold for 40-60 minutes; after exiting the furnace, easily crackable steel or steel with an alloy content of more than 20% should be cooled in an electroslag ingot for 12-24 hours, while other steel grades should be air-cooled.
[0012] In the above technical solution, further, the multifunctional protective atmosphere vacuum pressurized electroslag furnace described in step ① has a coaxial conductive function, upper and lower furnace chambers, and can place the crystallizer into the lower furnace chamber. It is equipped with a meshing device and an oxygen detection instrument. Using the multifunctional protective atmosphere vacuum pressurized electroslag furnace, its coaxial conductive function can achieve electromagnetic stirring opposite to the movement of the molten steel in the furnace, achieving a uniform composition. Its upper and lower furnace chambers, along with the dedicated meshing device for sealing, provide excellent airtightness. The rapid introduction of argon gas as a protective atmosphere into the furnace and the quick removal of air from the furnace ensure that all oxygen is expelled, resulting in good argon protection and controlling the oxygen level in the furnace to 0 ppm. Simultaneously, the rational use of refining slag with low residual oxide content (SiO2 ≤ 0.01%, FeO ≤ 0.003%) can effectively prevent the large-scale burn-off of easily oxidized elements such as Al and Ti in electroslag ingots containing Al, Ti, or both. The burn-off amount can be controlled within ≤ 8%, and the deviation of Al and Ti content in the upper and lower parts of the electroslag ingot can be stably controlled within ≤ 5%, ensuring the uniformity of Al and Ti content in the electroslag ingot.
[0013] Furthermore, the consumable electrode mentioned in step ① can be a billet produced by various smelting methods, such as a vacuum induction ingot, a continuous casting billet, or a die-casting billet, with a specification of ∮100mm and an electroslag ingot with a production ingot shape of ∮150mm.
[0014] Furthermore, in step ①, the FeO on the surface of the consumable electrode is first peeled off by turning or shot blasting to remove rust.
[0015] Furthermore, the slag mentioned in step ① is refined slag, whose main components by mass content are CaF2: 65-70%, Al2O3: 25-30%, MgO: 2-5%, SiO2≤0.01%, FeO≤0.003%, H2O≤0.5%. The TiO2 content is appropriately adjusted according to the specific steel grade, and the CaF2 and Al2O3 contents are reduced; the slag amount is 3-4 kg / furnace.
[0016] Furthermore, the smelting method for the refined slag is as follows: A 3-ton ordinary pressure electroslag remelting furnace is used, with a slag weight of 150 kg / furnace. Fe-Al electrodes are used as the smelting electrodes. During the smelting process, CaF2 and Al2O3 are first added to the furnace in batches to initiate arc formation and slag building. After a certain molten pool is formed, MgO and TiO2 are added to the furnace to form more slag. After the slag addition is complete, Al powder is added at a rate of 360–400 g / 5 min, totaling 5–6.5 kg. The refining time is 70–80 min. The Fe-Al electrode has an Al content of 4.5–5.5% by mass, a Mn content of 0.3–0.5% by mass, and the remainder is Fe.
[0017] Furthermore, the slag mentioned in step ① is dried by baking until it is red-hot, at a baking temperature of 800-950℃, and for a baking time of more than 12 hours.
[0018] Furthermore, the high-purity argon gas mentioned in step ③ has an Ar content of 99.999%.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0020] This invention employs a multifunctional protective atmosphere vacuum pressurized electroslag furnace. Its coaxial conductive function enables electromagnetic stirring that is opposite to the movement of the molten steel inside the furnace, achieving the technical effect of uniform steel composition. This specific equipment can control the oxygen content in the furnace to 0 ppm. By rationally using refining slag with low residual oxide content (SiO2 ≤ 0.01%, FeO ≤ 0.003%), it can effectively prevent the large-scale burn-off of easily oxidized elements such as Al and Ti in electroslag ingots containing Al and Ti. The burn-off amount can be controlled within 8%, and the deviation of Al and Ti content in the upper and lower parts of the electroslag ingot can be stably controlled to ≤ 5%, ensuring the uniformity of Al and Ti content in the electroslag ingot. Detailed Implementation
[0021] The present invention will be further described below with reference to specific embodiments, but this does not limit the invention in any way. To avoid redundancy, unless otherwise specified, the raw materials used in the following embodiments are all commercially available products, and the methods used are all conventional methods unless otherwise specified.
[0022] Example 1
[0023] The technical solution of this invention is used to produce 38CrMoAlA for military use. The composition of the 38CrMoAlA billet is shown in Table 1.
[0024] Table 1 Composition of 38CrMoAlA billet
[0025] C% Si% Mn% P% S% Al% Cr% Co% Ni% Cu% Ti% O% 0.40 0.31 0.48 0.014 0.008 1.0 1.47 0.06 0.23 0.07 0.02 0.0018
[0026] A method for controlled aluminum and titanium electroslag remelting under an oxygen-free protective atmosphere, the method comprising the following technical solutions:
[0027] ① The process is carried out using a 50 kg multi-functional protective atmosphere vacuum pressure electroslag furnace with upper and lower furnace chambers, a meshing device for good sealing, the ability to place the crystallizer into the lower furnace chamber, oxygen detection instruments, and coaxial conductivity. The consumable electrode and slag are pretreated: the billet (consumable electrode) used is a continuously cast billet with a specification of ∮100 mm, and the produced ingot is an electroslag ingot with a specification of ∮150 mm. The FeO on the surface of the consumable electrode must be removed by turning or shot blasting.
[0028] The slag is refined slag, and its main components are CaF2:Al2O3:MgO = 65:30:5, SiO2 ≤ 0.01%, FeO ≤ 0.003%, H2O ≤ 0.05%; the slag quantity is 3 kg / furnace.
[0029] The refining slag is produced using a 3-ton ordinary pressure electroslag furnace, with a slag weight of 150 kg / furnace. The smelting electrode is an Fe-Al electrode (Al content 4.5%, Mn content 0.5%, and the remainder Fe). During the smelting process, CaF2 and Al2O3 are first added to the furnace in batches to initiate the arc and form slag. After a certain molten pool is formed, MgO is added to the furnace to form slag. After the slag is added, Al powder is added at a rate of 360 g / 5 min, for a total of 5 kg. The refining time is 70 min.
[0030] The slag is heated until red-hot and dried at a temperature of 950°C for more than 12 hours.
[0031] ② The basic electrical system for electroslag is a voltage of 20-50V and a current of 700-4500A; conductive slag containing TiO2 is added for arc initiation; the ingot ignition plate is made of the same steel as the electroslag ingot and is derusted using a laser rust removal machine.
[0032] ③ At the start of electroslag remelting, high-purity argon gas (Ar content 99.999%) is first introduced, and the oxygen detection equipment is turned on to reduce the oxygen in the furnace to 0 ppm; after the oxygen in the furnace is reduced to 0 ppm, arc ignition and slag formation are started, with the voltage controlled at 20-45V and the current controlled at 700-2850A.
[0033] ④ After slag formation is completed, the oxygen level in the furnace will drop to 0 ppm again (during slag formation, the slag material and consumable electrodes will produce decomposed oxygen), and then electroslag refining will begin. During the electroslag refining period, the voltage will be controlled at 30-32V and the current at 2400-2750A. During the feeding period, the time will be controlled within 5 minutes, the voltage will remain unchanged, and the current will decrease by 700A per minute until it reaches 0A.
[0034] ⑤ Power off and cool the mold for 60 minutes; after removing from the oven, air cool.
[0035] The 38CrMoAlA electroslag ingot produced using Example 1 of this method has good surface quality, is free from defects such as arcing, waistlines, and slag inclusions, and exhibits good feeding effect. Its specific composition is shown in Table 2 below.
[0036] Table 2. Composition content of 38CrMoAlA electroslag ingots produced in Example 1
[0037] Location C% Si% Mn% P% S% Al% Cr% Co% Ni% Cu% Ti% O% upper part 0.40 0.30 0.49 0.014 0.005 0.97 1.48 0.06 0.24 0.06 0.02 0.0015 lower part 0.39 0.32 0.47 0.015 0.006 0.95 1.47 0.06 0.21 0.07 0.06 0.0017
[0038] The Al content loss in the upper part of the electroslag ingot is 3%, and the Al content loss in the lower part is 5%, with a compositional deviation of less than 2%. Ti in the electroslag ingot is a residual element and not an element that needs to be controlled, so it is not compared.
[0039] Example 2
[0040] The technical solution of this invention is used to produce stainless steel 06Cr18Ni11Ti. The composition of the 06Cr18Ni11Ti billet is shown in Table 3.
[0041] Table 3 Composition of 06Cr18Ni11Ti billet
[0042] C% Si% Mn% P% S% Cr% Ni% Ti% O% 0.05 0.56 1.45 0.012 0.006 17.56 10.2 0.65 0.0017
[0043] A method for controlled aluminum and titanium electroslag remelting under an oxygen-free protective atmosphere, the method comprising the following technical solutions:
[0044] ① The process is carried out using a 50 kg multi-functional protective atmosphere vacuum pressure electroslag furnace with upper and lower furnace chambers, a meshing device for good sealing, the ability to place the crystallizer into the lower furnace chamber, oxygen detection instruments, and coaxial conductivity. The consumable electrode and slag are pretreated: the billet (consumable electrode) used is a die-casting billet with a specification of ∮100 mm, and the produced ingot is an electroslag ingot with a size of ∮150 mm. The FeO on the surface of the consumable electrode is first shot-blasted to remove rust.
[0045] The slag is refined slag, and its main components are in the following mass ratio: CaF2:Al2O3:MgO:TiO2 = 70:25:4.5:0.5, SiO2 ≤ 0.01%, FeO ≤ 0.003%, H2O ≤ 0.05%; the slag amount is 3.5 kg / furnace.
[0046] The refining slag is produced using a 3-ton ordinary pressure electroslag furnace, with a slag weight of 150 kg / furnace. The smelting electrode is an Fe-Al electrode (Al content 5.5%, Mn content 0.5%, and the remainder Fe). During the smelting process, CaF2 and Al2O3 are first added to the furnace in batches to initiate the arc and form slag. After a certain molten pool is formed, MgO and TiO2 are added to the furnace to form slag. After the slag is added, 400 g of Al powder is added every 5 minutes, for a total of 6 kg. The refining time is 75 minutes.
[0047] The slag is heated until red-hot and dried at a temperature of 900°C for 14 hours.
[0048] ② The basic electrical system for electroslag is a voltage of 20-50V and a current of 700-4500A; conductive slag containing TiO2 is added for arc initiation; the ingot ignition plate is made of the same steel as the electroslag ingot and is derusted using a laser rust removal machine.
[0049] ③ At the start of electroslag remelting, high-purity argon gas (Ar content 99.999%) is first introduced, and the oxygen detection equipment is turned on to reduce the oxygen in the furnace to 0 ppm; after the oxygen in the furnace is reduced to 0 ppm, arc ignition and slag formation are started, with the voltage controlled at 20-45V and the current controlled at 700-2850A.
[0050] ④ After slag formation is completed, the oxygen level in the furnace will drop to 0 ppm again (during slag formation, the slag material and consumable electrodes will produce decomposed oxygen), and then electroslag refining will begin. During the electroslag refining period, the voltage will be controlled at 30-32V and the current at 2400-2450A. During the feeding period, the time will be controlled within 5 minutes, the voltage will remain unchanged, and the current will decrease by 500A per minute until it reaches 0A.
[0051] ⑤ After power failure, allow the mold to cool for 50 minutes; after removing from the oven, allow it to cool in the drum for 12 hours.
[0052] The 06Cr18Ni11Ti stainless steel electroslag ingot produced using Example 2 of this method has good surface quality, is free from defects such as arcing, waistlines, and slag inclusions, and exhibits good feeding effect. The specific composition of the upper and lower parts of this 06Cr18Ni11Ti stainless steel electroslag ingot is shown in Table 4.
[0053] Table 4. Composition of stainless steel 06Cr18Ni11Ti electroslag ingots produced in Example 2.
[0054] Location C% Si% Mn% P% S% Cr% Ni% Ti% O% upper part 0.05 0.55 1.45 0.012 0.003 17.57 10.2 0.62 0.0015 lower part 0.047 0.56 1.43 0.012 0.006 17.50 10.1 0.67 0.0016
[0055] The Ti content loss in the upper part of the electroslag ingot is about 4.6%, while the Ti content loss in the lower part is about 0%, with a deviation of 4.6% between the upper and lower parts.
[0056] Example 3
[0057] The high-temperature alloy GH4169 is produced using the technical solution of this invention. The composition of the GH4169 vacuum induction ingot billet is shown in Table 5, wherein the O content is 10 ppm.
[0058] Table 5 Composition of GH4169 Vacuum Induction Ingot Billet
[0059] C% Si% Mn% P% S% Al% Cr% Co% Ni% Cu% Ti% Mo% Fe% 0.04 0.31 0.18 0.009 0.003 0.70 17.72 0.06 50.5 0.04 0.86 2.95 27.8
[0060] A method for controlled aluminum and titanium electroslag remelting under an oxygen-free protective atmosphere, the method comprising the following technical solutions:
[0061] ① The process is carried out using a 50 kg multi-functional protective atmosphere vacuum pressure electroslag furnace with upper and lower furnace chambers, a meshing device for good sealing, the ability to place the crystallizer into the lower furnace chamber, oxygen detection instruments, and coaxial conductivity. The consumable electrode and slag are pretreated: vacuum induction ingots are used as consumable electrode blanks with a specification of ∮100 mm, and the produced ingots are ∮150 mm in size. The FeO on the surface of the consumable electrode is shot blasted to remove rust.
[0062] The slag is refined slag, and its main components are CaF2:Al2O3:MgO:TiO2 = 70:25:3:2, SiO2 ≤ 0.01%, FeO ≤ 0.003%, H2O ≤ 0.05%; the slag amount is 3.7 kg / furnace.
[0063] The refining slag is produced using a 3-ton ordinary pressure electroslag furnace, with a slag weight of 150 kg / furnace. The smelting electrode is an Fe-Al electrode (Al content 5.0%, Mn content 0.4%, and the remainder Fe). During the smelting process, CaF2 and Al2O3 are first added to the furnace in batches to initiate the arc and form slag. After a certain molten pool is formed, MgO and TiO2 are added to the furnace to form slag. After the slag is added, Al powder is added at a rate of 380 g / 5 min, for a total of 5.5 kg. The refining time is 70 min.
[0064] The slag was dried by baking at 950°C for 14 hours.
[0065] ② The basic electrical system for electroslag remelting is a voltage of 30-48V and a current of 700-4300A; conductive slag containing TiO2 is added for arc initiation; the ingot ignition plate is made of the same steel as the electroslag ingot and is rusted by shot blasting.
[0066] ③ At the start of electroslag remelting, high-purity argon gas (Ar content 99.999%) is first introduced, and the oxygen detection equipment is turned on to reduce the oxygen in the furnace to 0 ppm; after the oxygen in the furnace is reduced to 0 ppm, arc ignition and slag formation are started, with the voltage controlled at 30-45V and the current controlled at 750-2700A.
[0067] ④ After slag formation is completed, the oxygen level in the furnace will drop to 0 ppm again (during slag formation, the slag material and consumable electrodes will produce decomposed oxygen), and then electroslag refining will begin. During the electroslag refining period, the voltage will be controlled at 30-32V and the current at 2400-2440A. During the feeding period, the time will be controlled within 5 minutes, the voltage will remain unchanged, and the current will decrease by 500A per minute until it reaches 0A.
[0068] ⑤ Cool the mold for 60 minutes after power failure; after removing it from the oven, cool it in the barrel for 24 hours.
[0069] The GH4169 electroslag ingot produced using Example 3 of this method has good surface quality, is free from defects such as arcing, waistlines, and slag inclusions, and exhibits good feeding effect. The specific upper and lower components of the GH4169 electroslag ingot produced in Example 3 are shown in Table 6, and the O content in the electroslag ingot is 9 ppm.
[0070] Table 6. Composition of GH4169 electroslag ingots produced in Example 3.
[0071] Location C% Si% Mn% P% S% Al% Cr% Co% Ni% Cu% Ti% Mo% Fe% upper part 0.043 0.32 0.18 0.009 0.002 0.67 17.74 0.06 50.5 0.04 0.85 2.96 27.9 lower part 0.043 0.32 0.18 0.009 0.002 0.65 17.74 0.06 50.8 0.04 0.83 2.96 27.9
[0072] The Al content loss in the upper part of the electroslag ingot was 4.3%, and the Al content loss in the lower part was 7.1%, with a compositional deviation of less than 2.8%.
[0073] The Ti content loss in the upper part of the electroslag ingot is about 1.1%, and the Ti content loss in the lower part is about 3.4%, with a deviation of 2.3% between the upper and lower parts.
[0074] For anyone skilled in the art, many possible variations and modifications can be made to the technical solutions of this invention, or equivalent embodiments can be modified based on the disclosed technical content, without departing from the scope of the technical solutions of this invention. Therefore, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of this invention without departing from the content of the technical solutions of this invention should still fall within the protection scope of the technical solutions of this invention.
Claims
1. A method for controlled aluminum and titanium electroslag remelting under an oxygen-free protective atmosphere, characterized in that, The method includes the following technical solutions: ① The process is carried out using a multi-functional protective atmosphere vacuum pressure electroslag furnace, and the consumable electrodes and slag are pretreated. ② The basic electrical system for electroslag remelting is a voltage of 20~50 V and a current of 700~4500 A; conductive slag containing TiO2 is added to initiate the arc according to the composition of the smelting steel; the ingot ignition plate is made of the same steel as the electroslag ingot and is rusted by shot blasting or laser rust removal machine. ③ When the electroslag remelting smelting begins, high-purity argon gas is first introduced, and the oxygen detection equipment is turned on to reduce the oxygen in the furnace to 0 ppm; after the oxygen in the furnace is reduced to 0 ppm, the arc ignition and slag formation are started, and the voltage is controlled at 20~46 V and the current is controlled at 700~2900 A. ④ After slag formation is completed and the oxygen level in the furnace reaches 0 ppm again, electroslag refining begins; during the electroslag refining period, the voltage is controlled at 30~32V and the current is controlled at 2400~2750 A; during the feeding period, the time is controlled within 5 minutes, the voltage remains unchanged, and the current decreases by 500~700 A per minute. ⑤ Power off and cool in mold for 40-60 minutes; after exiting the furnace, easily crackable steel or steel with an alloy content of more than 20% should be cooled in an electroslag ingot for 12-24 hours, while other steel grades should be air-cooled. The multifunctional protective atmosphere vacuum pressurized electroslag furnace described in step ① has coaxial conductivity, upper and lower furnace chambers, and can place the crystallizer into the lower furnace chamber. It is equipped with a meshing device and an oxygen detection instrument. The slag mentioned in step ① is refined slag, and its main components by mass content are CaF2: 65~70%, Al2O3: 25~30%, MgO: 2~5%, SiO2≤0.01%, FeO≤0.003%, H2O≤0.5%; the slag amount is 3~4 kg / furnace.
2. The method according to claim 1, characterized in that, The consumable electrode mentioned in step ① is a vacuum induction ingot, a continuous casting billet, or a die-casting billet with a specification of ∮100 mm, and an electroslag ingot with a production ingot shape of ∮150 mm.
3. The method according to claim 1, characterized in that, In step ①, the FeO on the surface of the consumable electrode is first peeled off by turning or shot blasting to remove rust.
4. The method according to claim 1, characterized in that, The refining slag is produced using a 3-ton ordinary pressure electroslag furnace with a slag weight of 150 kg / furnace. Fe-Al electrodes are used for the smelting process. During the smelting process, CaF2 and Al2O3 are first added to the furnace in batches to initiate the arc and form slag. After a certain molten pool is formed, MgO and TiO2 are added to the furnace to form slag. After the slag is added, Al powder is added at a rate of 360-400 g / 5 min, for a total of 5-6.5 kg. The refining time is 70-80 min.
5. The method according to claim 4, characterized in that, The Fe-Al electrode has an Al content of 4.5-5.5%, a Mn content of 0.3-0.5%, and the remainder is Fe.
6. The method according to claim 1, characterized in that, The slag described in step ① is dried by baking until it turns red, at a baking temperature of 800~950℃, for a baking time of more than 12 hours.
7. The method according to claim 1, characterized in that, The high-purity argon gas mentioned in step ③ has an Ar content of 99.999%.
Citation Information
Patent Citations
Mold steel electroslag re-melting slag system and use method of mold steel electroslag re-melting slag system
CN102605190A
Low-aluminum high-titanium type high-temperature alloy electroslag remelting process
CN108660320A