Magnesium alloy modified conversion solution and magnesium alloy conversion treatment method

The modified conversion solution, composed of rare earth salts, sulfates, complexing agents, and surfactants, simplifies the preparation process of magnesium alloy conversion films, solves the problem of cumbersome traditional processes, achieves good bonding between the film layer and the substrate and improves corrosion resistance, and is suitable for surface treatment of magnesium alloys.

CN118127496BActive Publication Date: 2026-11-24ZHENGZHOU UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410071682.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-17
Publication Date
2026-11-24
Estimated Expiration
2044-01-17

AI Technical Summary

Technical Problem

Existing magnesium alloy conversion coating preparation processes are cumbersome, requiring complex pretreatment and post-treatment, and the film layer has poor adhesion to the substrate and insufficient corrosion resistance, making it difficult to meet practical needs.

Method used

A modified conversion solution composed of rare earth salts, sulfates, complexing agents and surfactants is used to form a uniform and dense film on a magnesium alloy substrate through simple grinding and room temperature treatment, omitting the traditional pretreatment steps.

Benefits of technology

Without pretreatment, a uniform and complete film layer is formed on the surface of magnesium alloy, which significantly improves corrosion resistance, is low in cost, environmentally friendly, and easy to industrialize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118127496B_ABST
    Figure CN118127496B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of alloy materials technology, and particularly relates to a magnesium alloy modification conversion solution, comprising rare earth salts, sulfates, complexing agents, and surfactants. The weight ratio of the rare earth salts to sulfates is 1.9-2.86; the weight ratio of the rare earth salts to the complexes is 3-7; and the weight ratio of the rare earth salts to the surfactants is 5-10. Using the magnesium alloy modification conversion solution of this invention, a uniform and dense film can be obtained on a substrate without pretreatment. The film has good adhesion to the substrate; even if the substrate has been corroded, the film can still bond tightly to the substrate. The conversion process is simple to operate, low in cost, and produces a white film that is uniform, has good corrosion resistance, and exhibits stable performance of both raw materials and finished products, making it easy to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of alloy materials technology, and particularly relates to a magnesium alloy modification conversion liquid and a magnesium alloy conversion treatment method. Background Technology

[0002] Magnesium alloys are lightweight metals, hailed as green and environmentally friendly materials of the 21st century. They possess advantages such as low density, high specific strength, good toughness, strong electromagnetic shielding ability, strong shock absorption, low heat capacity, fast solidification speed, good machinability, easy recycling, and no pollution. They can be used in the automotive industry to accelerate the development of lightweight vehicles, and also in aerospace, components for important weapons, and the computer and electronics industries, with a wide range of applications. However, magnesium alloys have low electrode potential and reactive chemical properties. The naturally formed oxide film on their surface has a PB ratio of less than 1, lacking the dense and protective oxide film of aluminum. This limits the application and service life of magnesium, leading to extensive research on corrosion resistance of magnesium alloys.

[0003] Chemical conversion coating is a simple surface treatment method that requires minimal equipment and low energy consumption. The process involves immersing a magnesium alloy in a prepared film-forming solution. Under specific temperature, pH, and time conditions, the magnesium alloy and the solution are allowed to fully react and react, depositing a layer of metal oxide on the magnesium alloy surface. This thin film provides good protection for the magnesium alloy and effectively improves its corrosion resistance. In typical practical applications, the chemical conversion coating is often used as a base coat, so it also needs to bond well with subsequent coatings.

[0004] Since the development of chromium-free technology, processing technologies such as phosphate conversion membranes, stannate conversion membranes, and rare earth conversion membranes have emerged. Rare earth conversion membranes, as environmentally friendly and corrosion-resistant membranes, have attracted much attention. Chinese patents CN105734550A and CN108456884B both disclose a pretreatment method for rare earth conversion films on magnesium alloys. Preparing the conversion film requires a series of cumbersome pretreatment processes. Chinese patents CN104357832A and CN101886258A both disclose methods for preparing magnesium alloy conversion films, but both require metal pretreatment processes such as degreasing and alkaline washing, while also introducing a magnetic field, increasing the cost of film formation. The steps are cumbersome and difficult to meet practical needs. Chinese patent CN114388068A discloses a method for preparing ternary rare earth conversion films. This method requires lengthy and complex calculations to determine the rare earth solution ratio, and the actual rare earth element content ratio in the final film is difficult to control, making it unsuitable for commercialization. Chinese patent CN1752287A discloses a method for improving the corrosion resistance of rare earth conversion films on the surface of light metals and their composite materials. The materials treated by this method need to be placed at room temperature for 15 days or heated in a drying oven at 40-80℃ for 1-24 hours, a complex and time-consuming process. Summary of the Invention

[0005] To solve the above-mentioned technical problems, the inventors improved the formulation of the magnesium alloy modification conversion solution, so that a uniform and dense film layer can be obtained on the magnesium alloy substrate without pretreatment, and the film layer has good adhesion to the substrate, thus completing the present invention.

[0006] Therefore, in a first aspect, the present invention provides a magnesium alloy modification conversion liquid comprising rare earth salts, sulfates, complexing agents and surfactants, wherein the weight ratio of the rare earth salts to sulfates is 1.9-2.86, preferably 2.28; the weight ratio of the rare earth salts to the complexes is 3-7, preferably 6; and the weight ratio of the rare earth salts to the surfactants is 5-10, preferably 7.

[0007] In a preferred embodiment, the magnesium alloy modification conversion solution comprises 50-60 parts by weight of rare earth salt, 25-30 parts by weight of sulfate, 6-10 parts by weight of complexing agent, and 6-8 parts by weight of surfactant; more preferably, the magnesium alloy modification conversion solution comprises 56.5 parts by weight of rare earth salt, 25 parts by weight of sulfate, 9 parts by weight of complexing agent, and 7.5 parts by weight of surfactant.

[0008] In some embodiments, the magnesium alloy modification conversion solution is composed of rare earth salts, sulfates, complexing agents and surfactants. Preferably, the magnesium alloy modification conversion solution is composed of 56.5 parts by weight of rare earth salts, 25 parts by weight of sulfates, 9 parts by weight of complexing agents and 7.5 parts by weight of surfactants.

[0009] In a preferred embodiment, the rare earth salt is selected from one or more of lanthanum nitrate, cerium nitrate, and yttrium nitrate, with lanthanum nitrate being preferred.

[0010] In a preferred embodiment, the sulfate is selected from one or more of sodium sulfate, magnesium sulfate, and potassium sulfate, preferably sodium sulfate or magnesium sulfate.

[0011] In a preferred embodiment, the complexing agent is selected from one or more of disodium ethylenediaminetetraacetate and potassium sodium tartrate, preferably disodium ethylenediaminetetraacetate.

[0012] In a preferred embodiment, the surfactant is selected from one or more of sodium dodecylbenzenesulfonate, fatty acid glycerides, and sodium α-alkenylsulfonate, preferably sodium dodecylbenzenesulfonate.

[0013] In a second aspect, the present invention provides a method for preparing the magnesium alloy modified conversion solution, comprising: pouring rare earth salt, sulfate, complexing agent and surfactant into deionized water, stirring to dissolve, and adjusting the pH to 4-5 with nitric acid to obtain the magnesium alloy modified conversion solution.

[0014] In a third aspect, the present invention provides a magnesium alloy conversion method, comprising the following steps:

[0015] S1 Substrate Preparation: Cut the magnesium alloy sample into specimens, and polish the surface of the specimens in sequence with 120#, 400#, 1200# and 2000# sandpaper, and rinse with alcohol and air dry.

[0016] S2 Conversion Treatment: The sample is suspended in the magnesium alloy modification conversion solution and converted at room temperature for 20 minutes. After the conversion treatment, it is immediately rinsed with deionized water and the surface is dried.

[0017] This invention uses sandpaper of different grits to polish the metal surface sequentially, starting with coarse sandpaper and gradually moving to fine sandpaper. This effectively removes surface oxides and makes the metal surface smooth, facilitating subsequent film formation.

[0018] Technical effect

[0019] Traditional magnesium alloy rare earth conversion coating preparation processes involve a series of cumbersome pretreatment steps. Some processes even introduce magnetic fields, long-term placement, or heating to improve the adhesion between the film and the substrate, significantly diminishing the fundamental advantages of chemical conversion coatings as a base layer—simple operation, basic equipment requirements, and low energy consumption. However, this invention, by adjusting the magnesium alloy modified conversion solution formula, eliminates the need for complex pretreatment and post-treatment, enabling the preparation of a conversion film with excellent adhesion to the substrate.

[0020] Using the magnesium alloy modification conversion solution of the present invention, the substrate can be simply polished without the need for pretreatment steps such as degreasing, cleaning, and activation to form a high-performance film on its surface. Compared with traditional rare earth conversion films, the film is uniform and complete, not easy to fall off, and has a significantly improved corrosion resistance.

[0021] Using the magnesium alloy modification conversion solution of this invention, a uniform film can be formed even on the surface of corroded magnesium alloys. The conversion process is simple to operate, low in cost, produces a white, uniform film with good corrosion resistance, and exhibits stable performance of both raw materials and finished products, making it easy to industrialize.

[0022] The film-forming treatment solution of this invention is free of phosphorus and chromium, environmentally friendly, low in cost, produces a white, uniform film with good corrosion resistance, and features stable performance of both raw materials and finished products, making it easy to industrialize. Attached Figure Description

[0023] Figure 1 The images show the surface and cross-sectional morphology of the modified magnesium alloy conversion film in Example 5 of this invention.

[0024] Figure 2 This is a schematic diagram of the hydrogen evolution weight loss device used in Embodiment 6 of the present invention;

[0025] Figure 3The results of hydrogen evolution experiments in 3.5 wt.% NaCl are shown for the membranes obtained using the treatment solutions of Comparative Example 1 and Example 1 in Example 6 of the present invention.

[0026] Figure 4 The cross-sectional morphology of the film obtained in Example 7 of the present invention after immersion in 3.5 wt.% NaCl etching solution for 7 days is shown;

[0027] Figure 5 The results of the film adhesion test in Example 8 of the present invention are shown. Detailed Implementation

[0028] The following description, with reference to the accompanying drawings, illustrates several preferred embodiments of the present invention to make its technical content clearer and easier to understand. The present invention can be embodied in many different forms, and the scope of protection of the present invention is not limited to the embodiments mentioned herein.

[0029] Example 1

[0030] The preparation of a magnesium alloy modification conversion solution involves weighing 11.3g of lanthanum nitrate, 5g of sodium sulfate, 1g of disodium ethylenediaminetetraacetate, 0.8g of potassium sodium tartrate, and 1.5g of sodium α-alkenyl sulfonate; accurately measuring 800mL of deionized water and pouring it into a 1000mL beaker; adding the above raw materials sequentially to the beaker and stirring until completely dissolved; adjusting the pH to 5 with nitric acid; and adding deionized water to 1000mL to obtain the magnesium alloy modification conversion solution.

[0031] Example 2

[0032] The preparation of a magnesium alloy modification conversion solution involves weighing 6.7g of lanthanum nitrate, 3g of sodium sulfate, 0.3g of disodium ethylenediaminetetraacetate, 0.6g of potassium sodium tartrate, and 1g of sodium dodecylbenzenesulfonate; accurately measuring 800mL of deionized water and pouring it into a 1000mL beaker; adding the above raw materials sequentially to the beaker and stirring until completely dissolved; adjusting the pH to 4.5 with nitric acid; and adding deionized water to 1000mL to obtain the magnesium alloy modification conversion solution.

[0033] Example 3

[0034] The preparation of a magnesium alloy modification conversion solution involves weighing 8g of lanthanum nitrate, 3.9g of sodium sulfate, 1g of disodium ethylenediaminetetraacetate, 0.5g of potassium sodium tartrate, and 0.9g of sodium dodecylbenzenesulfonate; accurately measuring 800mL of deionized water and pouring it into a 1000mL beaker; adding the above raw materials sequentially to the beaker and stirring until completely dissolved; adjusting the pH to 4 with nitric acid; and adding deionized water to 1000mL to obtain the magnesium alloy modification conversion solution.

[0035] Example 4

[0036] The preparation of a magnesium alloy modification conversion solution involves weighing 12g of lanthanum nitrate, 5.8g of sodium sulfate, 1g of disodium ethylenediaminetetraacetate, 0.6g of potassium sodium tartrate, and 1.5g of fatty acid glycerides; accurately measuring 800mL of deionized water and pouring it into a 1000mL beaker; adding the above raw materials sequentially to the beaker and stirring until completely dissolved; adjusting the pH to 5 with nitric acid; and adding deionized water to 1000mL to obtain the magnesium alloy modification conversion solution.

[0037] Example 5

[0038] A method for converting magnesium alloys:

[0039] S1: Cut EW75 magnesium alloy into 20×20×10mm samples, drill a hole in one corner of the sample, and polish the sample surface in turn with 120#, 400#, 1200# and 2000# sandpaper respectively, and rinse with alcohol and air dry.

[0040] S2: After polishing, surface activation and cleaning are not required. The sample is directly suspended with cotton thread and placed into the magnesium alloy modification conversion solution prepared in Example 1 for conversion treatment. The conversion temperature is room temperature and the time is 20 minutes. After the conversion treatment, the sample is immediately rinsed with deionized water and the surface is dried with a hair dryer.

[0041] The surface morphology of the samples was directly captured by dual-beam electron microscopy (SEM). For the cross-sectional morphology, a 10mm x 10mm x 10mm sample was first deposited into a film, placed in a mold, sealed with epoxy resin, and after solidification, the surface was polished before observation using an SEM. The surface and cross-sectional morphology images of the converted magnesium alloy film are shown below. Figure 1 As shown in the figure, the film layer has a cracked, soil-like appearance, is dense and uniform, and does not expose the bare metal substrate. The cracks are likely caused by residual stress generated during drying.

[0042] Using the same magnesium alloy conversion method as in Example 5, similar conversions can be achieved using the magnesium alloy modified conversion solutions prepared in Examples 2-4, and a uniform and dense white film can be formed on the untreated metal surface.

[0043] Comparative Example 1

[0044] To prepare the traditional rare earth conversion solution, weigh 8g of lanthanum nitrate and 1000mL of deionized water, and stir until completely dissolved to obtain the traditional lanthanum rare earth conversion solution.

[0045] The magnesium alloy conversion method consists of the following steps:

[0046] S1 Substrate Preparation: Cut EW75 magnesium alloy into 20×20×10mm samples, drill a hole at one corner of the sample, polish the sample surface with 120#, 400#, 1200# and 2000# sandpaper respectively, rinse with alcohol and air dry.

[0047] S2 Surface Activation: The polished sample is immersed in alcohol and sonicated for 20 minutes to clean and degrease the surface. After removal, it is rinsed with deionized water and then immersed in an alkaline cleaning solution for 15 minutes. The alkaline solution consists of 1.5g NaOH, 1g Na3PO4·12H2O, 1.5g Na2CO3, and 100mL deionized water. The sample is then removed and rinsed with deionized water. It is then immersed in an acid solution for activation for 2 minutes. After removal, it is rinsed with deionized water. The acid solution consists of 1mL H2SO4, 1mL HNO3, 3mL citric acid, and 500mL deionized water.

[0048] S3 Conversion Treatment: The sample after the above treatment is suspended by cotton thread and placed in the prepared rare earth conversion solution for conversion treatment. The conversion temperature is room temperature and the time is 20 minutes. After the conversion treatment, the sample is immediately rinsed with deionized water and the surface is dried with a hair dryer.

[0049] Example 6: Hydrogen evolution experiment

[0050] The experimental sample was a standard block of 20mm*20mm*10mm. A hole was drilled in the upper left corner of the sample. All six sides were sanded with sandpaper to 2000#. The sample was rinsed with alcohol and treated with the magnesium alloy modification conversion solution prepared in Example 1 to form a film. The dimensions were measured and the total area S of the six sides was calculated.

[0051] Adopting such Figure 2 The experimental setup shown suspends the sample block in a 3.5 wt.% sodium chloride solution, avoiding contact with the bottom of the beaker and the wall of the funnel.

[0052] Read the initial value L0 from the burette, and then read the value L again after a certain time interval. x After soaking, the recorded values ​​will be plotted and calculated.

[0053] According to the formula Calculate the amount of hydrogen evolution V at different soaking times. h and with V h A hydrogen evolution comparison chart is plotted with the vertical axis representing the hydrogen evolution time and the horizontal axis representing the hydrogen evolution time. According to the formula... Calculate the annual corrosion rate, where P h Annual corrosion rate (mm·year) -1 M is the relative atomic mass (g·mol⁻¹) -1 ), ΔV h Hydrogen evolution rate V for different soaking times hThe difference (mL·cm) -2 ·d -1 ), where n is the number of electrons lost by the atom, and ρ is the metal density (g·cm³). -3 ).

[0054] The hydrogen evolution results of the conventional rare earth conversion membrane prepared in Comparative Example 1 and the modified rare earth conversion membrane prepared in Example 1 in 3.5 wt.% sodium chloride solution are as follows: Figure 3 As shown in the figure. The annual corrosion rate of the modified rare earth conversion film is calculated to be 0.23 mm / year, while that of the traditional rare earth conversion film is 0.407 mm / year. It can be seen that the modified film obtained by treatment with the magnesium alloy modified conversion solution prepared in Example 1 of this invention exhibits a significantly reduced hydrogen evolution rate and a reduced amount of hydrogen evolution, indicating a significant improvement in corrosion resistance.

[0055] Example 7: Total Immersion Experiment

[0056] A magnesium alloy sample with dimensions of 10mm*10mm*10mm was drilled and all six sides were polished. The sample was then treated with the magnesium alloy modification conversion solution prepared in Example 1 to form a film. After film formation, the sample was suspended and immersed in a 3.5wt.% sodium chloride solution. After 7 days of corrosion, the sample was removed and the corrosion cross section between the film and the substrate was observed.

[0057] The cross-sectional morphology of the film corrosion after 7 days of full immersion experiment is as follows Figure 4 As shown, although some of the substrate was corroded, the film layer remained tightly bonded and showed no signs of detachment. Furthermore, after seven days of immersion, the film layer showed no corrosion, providing continuous protection for the metal.

[0058] Example 8: Adhesion Test

[0059] The bonding strength between the film and the magnesium alloy substrate was studied using adhesive tape experiments.

[0060] First, the sample after the film layer was prepared in Example 5 was divided into 2mm×2mm areas using a cross-cutting tool. Then, the film layer was adhered and peeled off using special transparent tape. The adhesion of the film layer was characterized by the peeling off of the film layer.

[0061] The results of the conversion film adhesion test are as follows: Figure 5 As shown, (a) is the sample surface after film formation in Example 5 of the present invention, (b) is the sample surface after being cut with a cross-cutting tool, and (c) is the result of the adhesive tape adhesion and tearing treatment after being cut with a cross-cutting tool. Overall, the film layer remains intact and uniform within the grid, without exposing the magnesium alloy substrate surface. Therefore, it can be considered that the film layer has good adhesion to the substrate.

[0062] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A method for converting magnesium alloys, comprising the following steps: S1 Substrate Preparation: Cut the magnesium alloy sample into specimens, and polish the surface of the specimens in sequence with 120#, 400#, 1200# and 2000# sandpaper, and rinse with alcohol and air dry. S2 Conversion Treatment: The sample was suspended in the magnesium alloy modification conversion solution and converted at room temperature for 20 minutes. After the conversion treatment, it was immediately rinsed with deionized water and the surface was dried. The magnesium alloy in the sample was EW75 magnesium alloy; The magnesium alloy modification conversion solution is composed of 56.5 parts by weight of rare earth salt, 25 parts by weight of sulfate, 9 parts by weight of complexing agent and 7.5 parts by weight of surfactant; the complexing agent is selected from one or more of disodium ethylenediaminetetraacetate and sodium potassium tartrate. The pH of the magnesium alloy modification and conversion solution is 4-5.

2. The magnesium alloy conversion method according to claim 1, wherein, The rare earth salt is selected from one or more of lanthanum nitrate, cerium nitrate, and yttrium nitrate.

3. The magnesium alloy conversion method according to claim 1, wherein, The sulfate is selected from one or more of sodium sulfate, magnesium sulfate, potassium sulfate, and ammonium sulfate.

4. The magnesium alloy conversion method according to claim 1, wherein, The surfactant is selected from one or more of sodium dodecylbenzenesulfonate, fatty acid glycerides, and sodium α-alkenylsulfonate.

5. The magnesium alloy conversion method according to claim 1, wherein, The magnesium alloy modification conversion solution is prepared by the following method: rare earth salt, sulfate, complexing agent and surfactant are poured into deionized water, stirred and dissolved, and then the pH is adjusted to 4-5 with nitric acid to obtain the magnesium alloy modification conversion solution.

Citation Information

Patent Citations

  • Method for preparing conversion wear-resistance film layer on magnesium alloy surface

    CN101886258A

  • Method for preparing conversion film on surface of magnesium alloy and composite material with conversion film

    CN104357832A

  • Preparation method for magnesium alloy rare earth conversion coating

    CN105734550A

  • A pretreatment method for homogenizing chromium-free conversion coatings on magnesium alloys

    CN108456884B

  • Preparation method of magnesium alloy with ternary rare earth conversion films with different weight percentages on surface and obtained magnesium alloy

    CN114388068A