Blade and cutting tool

CN118139707BActive Publication Date: 2026-11-20KYOCERA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202280067075.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-10-29
Filing Date
2022-10-06
Publication Date
2026-11-20
Estimated Expiration
2042-10-06

Smart Images

  • Figure CN118139707B_ABST
    Figure CN118139707B_ABST
Patent Text Reader

Abstract

The insert (1) of the present disclosure has a base (2) and a coating (3) that coats the surface of the base (2). The base (2) is composed of a cermet. The coating (3) is composed of Ti 1‑a‑b‑c‑d Al a M b W c Si d (C x N 1‑x ), wherein the metal element M is one or more metal elements selected from Nb, Mo, Ta, Hf, Y, and 0.40 ≤ a ≤ 0.55, 0.01 ≤ b ≤ 0.1, 0.01 ≤ c ≤ 0.1, 0.01 ≤ d ≤ 0.05, 0 ≤ x ≤ 1. In addition, the insert (1) of one aspect of the present disclosure is provided with an intermediate layer (4) containing Ti between the base (2) and the coating (3). The average thickness of the intermediate layer (4) is 20 nm or more and 80 nm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to cutting blades and cutting tools. Background Technology

[0002] Titanium (Ti)-based cermets are widely used as the matrix for components that require wear resistance, lubrication, and chipping resistance, such as cutting tools, wear-resistant components, or lubrication components.

[0003] Patent document 1 discloses a metal-ceramic cutting tool in which a melt-separated alloy phase composed of metal binder phase components is disposed on the surface of a metal-ceramic matrix containing a binder phase component mainly composed of cobalt (Co) and nickel (Ni), and a TiN layer with diffusion prevention function is disposed on the melt-separated alloy phase.

[0004] Prior art literature

[0005] Patent documents

[0006] Patent Document 1: Japanese Patent No. 3099834 Summary of the Invention

[0007] One embodiment of the blade disclosed herein has a substrate and a coating applied to the surface of the substrate. The substrate is made of cermet. The coating is made of Ti. 1-a-b-c-d Al a M b W c Si d (C x N 1-x The substrate is composed of a substrate, wherein the metal element M is selected from one or more metal elements chosen from Nb, Mo, Ta, Hf, and Y, and the metal elements have the following properties: 0.40≤a≤0.55, 0.01≤b≤0.1, 0.01≤c≤0.1, 0.01≤d≤0.05, and 0≤x≤1. Furthermore, one embodiment of the blade disclosed herein has a Ti-containing intermediate layer disposed between the substrate and the coating. The average thickness of the intermediate layer is 20 nm or more and 80 nm or less. Attached Figure Description

[0008] Figure 1 This is a perspective view showing an example of the blade involved in the embodiment.

[0009] Figure 2 This is a side sectional view showing an example of the blade involved in the embodiment.

[0010] Figure 3 This is a schematic enlarged view of the cross-section of the intermediate layer.

[0011] Figure 4 This is a front view showing an example of a cutting tool involved in the implementation method.

[0012] Figure 5 It is a graph representing the results of hardness testing.

[0013] Figure 6 This is a graph showing the results of measuring the residual compressive stress of the coatings of samples No.1 to No.4.

[0014] Figure 7 It is a graph representing the results of the bonding strength measurement.

[0015] Figure 8 It is a table summarizing the results of hardness testing, stress testing, and bonding strength testing.

[0016] Figure 9 This is a diagram showing the Ti element mapping image in the intermediate layer of sample No.1.

[0017] Figure 10 This is a diagram showing the Ar element mapping image in the intermediate layer of sample No.1.

[0018] Figure 11 It is Figure 10 The table shows the elemental structure ratios at measurement points P1 to P4, expressed in atomic percent.

[0019] Figure 12 It is a graph representing the results of a wear test. Detailed Implementation

[0020] Hereinafter, the forms of the cutting blades and cutting tools used to implement the present disclosure will be described in detail with reference to the accompanying drawings (hereinafter referred to as "Embodiments"). It should be noted that the cutting blades and cutting tools of the present disclosure are not limited to these embodiments. Furthermore, the various embodiments can be appropriately combined within the scope where the content does not contradict each other. In addition, the same reference numerals are used to label the same parts in the following embodiments, and repeated descriptions are omitted.

[0021] Furthermore, in the embodiments shown below, expressions such as "constant," "orthogonal," "perpendicular," or "parallel" are sometimes used, but these expressions are not required to be strictly "constant," "orthogonal," "perpendicular," or "parallel." That is, the above expressions allow for deviations, such as manufacturing precision or setting precision.

[0022] Previously, it was known that the residual stress of the coating increased when a coating was formed on a cermet substrate. When the residual stress of the coating is high, it is prone to peeling off from the substrate, thus making it difficult to improve the wear resistance of the cutting tool. It should be noted that forming a low-hardness coating can reduce the residual stress of the coating. However, in doing so, the wear resistance of the coating itself decreases, thus making it difficult to improve the wear resistance of the cutting tool.

[0023] Given this situation, there is an expectation for the provision of cutting blades and cutting tools with excellent wear resistance.

[0024] <Blade>

[0025] Figure 1 This is a perspective view showing an example of the blade involved in the embodiment. Additionally, Figure 2 This is a side sectional view showing an example of the blade 1 according to the embodiment. For example... Figure 1 and Figure 2 As shown, the blade 1 involved in the embodiment has a substrate 2, a coating 3, and an intermediate layer 4.

[0026] (Matrix 2)

[0027] The substrate 2 has, for example, an upper surface and a lower surface ( Figure 1 The shape of the surface intersecting the Z-axis shown is a parallelogram-shaped hexahedron.

[0028] One corner of the base 2 functions as a cutting edge. The cutting edge has a first surface (e.g., an upper surface) and a second surface (e.g., a side surface) connected to the first surface. In an embodiment, the first surface functions as a "rake face" that picks up the chips generated by cutting, and the second surface functions as a "flank face". At least a portion of the edge where the first and second surfaces intersect is provided with a cutting edge, and the insert 1 cuts the workpiece by pressing such a cutting edge against the workpiece.

[0029] Alternatively, a through hole 21 can be provided in the center of the base 2, extending vertically through the base 2. In this case, a screw 75 for mounting the blade 1 to the tool holder 70 (described later) is inserted into the through hole 21. Figure 4 ).

[0030] Matrix 2 is composed of cermet. The cermet contains a hard layer and a binder phase. The hard layer may also contain Ti. For example, the hard layer may be mainly composed of at least one element selected from TiCN, TiC, TiN, TiMN (M is at least one metallic element selected from Groups 4, 5, and 6 of the periodic table, Al, and Si, excluding Ti). The binder phase is mainly composed of iron group metals such as Ni or Co. It should be noted that the main component can also be a component that accounts for more than 50% by mass of the constituent elements.

[0031] (Coating 3)

[0032] Coating 3 is applied to the substrate 2 for purposes such as improving its wear resistance and heat resistance. Figure 2The example shown illustrates a case where coating 3 covers the entire surface of substrate 2, but coating 3 does not necessarily need to cover the entire surface of substrate 2. When coating 3 is located on the first surface of substrate 2 (here, the upper surface), the first surface exhibits high wear resistance and heat resistance. When coating 3 is located on the second surface of substrate 2 (here, the side surface), the second surface exhibits high wear resistance and heat resistance.

[0033] Coating 3 may, for example, contain cubic crystals comprising: one or more elements selected from the group consisting of elements from Group 4, Group 5, Group 6, Si, and Al of the periodic table; and one or more elements selected from the group consisting of C, N, and O. With such a structure, the oxidation resistance of coating 3 is improved. Consequently, the wear resistance of coating 3 is further improved.

[0034] For example, coating 3 can also be a TiAlSiN layer containing Ti, Al, Si, and N. In this way, by placing coating 3, containing the metal (Ti) contained in intermediate layer 4, on top of intermediate layer 4, the adhesion between intermediate layer 4 and coating 3 is improved. Consequently, coating 3 is less likely to peel off from intermediate layer 4, thus improving the durability of coating 3. It should be noted that the term "TiAlSiN" refers to the presence of Ti, Al, Si, and N in any proportion, and does not necessarily mean that Ti, Al, Si, and N exist in a one-to-one, one-to-one, one-to-one configuration.

[0035] As a specific example, coating 3 could also be made of Ti. 1-a-b-c-d Al a M b W c Si d (C x N 1-x The layer is composed of Nb, Mo, Ta, Hf, and Y. Here, M is one or more metallic elements selected from the group consisting of Nb, Mo, Ta, Hf, and Y. Furthermore, a to d are 0.40≤a≤0.55, 0.01≤b≤0.1, 0.01≤c≤0.1, and 0.01≤d≤0.05, respectively, and x is 0≤x≤1.

[0036] Coating 3 can also have a hardness of 33.5 GPa or higher and a residual compressive stress of 1.4 GPa or lower. With this structure, the bonding force between the substrate 2 and coating 3 is further improved. Furthermore, the wear resistance of coating 3 is improved, thereby extending the life of the cutting tool 1.

[0037] The adhesion strength of coating 3 to substrate 2 (hereinafter referred to as "adhesion strength") can also achieve a peel load of 110 N or more in a scratch test. With this structure, the internal stress and thermal stress that determine the adhesion strength between substrate 2 and coating 3 are optimized, making coating 3 less prone to peeling while maintaining its high hardness. As a result, the blade 1 has a further extended lifespan.

[0038] (Coating manufacturing method)

[0039] Coatings can also be formed by physical vapor deposition, for example. Examples of physical vapor deposition methods include ion plating and sputtering. As an example, when using ion plating to create a coating, the coating can be created using the following method.

[0040] As an example, an example of a method for preparing a coating using ion plating is shown. First, as an example, metal targets, composite alloy targets, or sintered targets of Ti, Al, M (wherein the metal element M is one or more metal elements selected from Nb, Mo, Ta, Hf, Y), W, and Si are prepared.

[0041] Next, the target material, which serves as the metal source, is ionized by evaporation through arc discharge or glow discharge. The ionized metal is then reacted with nitrogen (N2) gas, a nitrogen source, and deposited onto the surface of the substrate. A coating can be formed through these steps.

[0042] Alternatively, the temperature of the substrate can be set to 500°C or higher and 600°C or lower, the nitrogen pressure can be set to 1.0 Pa or higher and 6.0 Pa or lower, and a DC bias voltage of -50 V or higher and -200 V or lower can be applied to the substrate to make the arc discharge current 100 A or higher and 200 A or lower.

[0043] The composition of the coating can be adjusted by independently controlling the voltage and current values ​​of the arc discharge and glow discharge applied to various metal targets for each target. Furthermore, the composition of the coating can also be adjusted by controlling the composition of the metal target, the coating time, and the atmospheric gas pressure.

[0044] (Middle layer 4)

[0045] An intermediate layer 4 may also be disposed between the substrate 2 and the coating 3. Specifically, the intermediate layer 4 is in contact with the upper surface of the substrate 2 on one side and with the lower surface of the coating 3 on the other side.

[0046] The intermediate layer 4 is mainly composed of Ti. The adhesion between this intermediate layer 4 and the substrate 2 is higher than the adhesion between the intermediate layer 4 and the coating 3. The proportion of Ti in the intermediate layer 4 can be determined, for example, by analysis using an EDS (energy-dispersive X-ray spectroscopy) instrument attached to a STEM (scanning transmission electron microscope).

[0047] Thus, the blade 1 involved in this embodiment has an intermediate layer 4 between the substrate 2 and the coating 3. The wettability between the intermediate layer 4 and the substrate 2 is higher than that between the intermediate layer 4 and the coating 3, resulting in high adhesion between the substrate 2 and the coating 3. It should be noted that the adhesion between the intermediate layer 4 and the coating 3 is also high, so it is not easy for the coating 3 to peel off from the intermediate layer 4.

[0048] The average thickness of the intermediate layer 4 can also be above 20 nm and below 80 nm. When the thickness of the intermediate layer 4 is above 20 nm, the bonding effect between the coating 3 and the substrate 2 is further enhanced. When the thickness of the intermediate layer 4 is below 80 nm, it can suppress the generation or intensification of cracks from the intermediate layer 4. Therefore, by making the average thickness of the intermediate layer 4 above 20 nm and below 80 nm, the bonding force between the substrate 2 and the coating 3 can be further improved, and the wear resistance and chipping resistance of the cutting tool 1 can be further improved.

[0049] The intermediate layer 4 involved in the embodiment may also contain Ar in addition to Ti. In the blade 1 with an intermediate layer 4 containing Ti and Ar between the substrate 2 and the coating 3, the adhesion between the substrate 2 and the coating 3 is higher.

[0050] Specifically, the intermediate layer 4 containing both Ti and Ar exhibits a higher stress mitigation effect compared to an intermediate layer containing only Ti (without Ar). The Ar-containing intermediate layer 4 effectively mitigates the abrupt stress changes from the substrate 2 to the coating 3. Consequently, the adhesion between the substrate 2 and the coating 3 can be considered improved.

[0051] Figure 3 This is a schematic enlarged view of the cross-section of intermediate layer 4. (See diagram below.) Figure 3 As shown, the intermediate layer 4 may also have multiple Ar-enriched regions 41. The Ar-enriched regions 41 are regions with a higher Ar content compared to other regions 42 of the intermediate layer 4. The presence of the Ar-enriched regions 41 can be determined, for example, by analysis using an EDS (energy-dispersive X-ray spectroscopy) instrument attached to a STEM (scanning transmission electron microscope).

[0052] Ar-rich regions 41 can also be distributed in an island-like pattern in the intermediate layer 4. Here, "island-like distribution" means that the Ar-rich regions 41 exist in an isolated state without touching each other. The shape of each Ar-rich region 41 is not particularly limited. For example, the Ar-rich region 41 can be a shape composed of curves, such as a circle or an ellipse, or a shape composed of straight lines, such as a polygon, or a shape composed of both curves and straight lines.

[0053] Thus, with multiple Ar-rich regions 41 distributed in an island-like pattern, the effect of mitigating the abrupt stress change from the substrate 2 to the coating 3 is further enhanced, thereby further improving the adhesion between the substrate 2 and the coating 3. As a result, the wear resistance and chipping resistance of the blade 1 are improved.

[0054] Regarding the multiple Ar enrichment regions 41, it is also possible that the Ar enrichment regions in region 4L of the intermediate layer 4 are more numerous than the Ar enrichment regions in region 4U of the intermediate layer 4. Region 4L is the region in the intermediate layer 4 that is closer to the substrate 2 than the center in the thickness direction (here, the Z-axis direction), and region 4U is the region in the intermediate layer 4 that is closer to the coating 3 than the center in the thickness direction.

[0055] Thus, with more Ar-rich regions 41 distributed in the thickness direction of the intermediate layer 4 compared to the region closer to the substrate 2, the abrupt change in stress from the substrate 2 to the intermediate layer 4 is mitigated, further enhancing the bonding force between the substrate 2 and the intermediate layer 4, and consequently, further enhancing the bonding force between the substrate 2 and the coating 3. As a result, the wear resistance and chipping resistance of the blade 1 are improved.

[0056] Ar-rich region 41 may also contain more than 3 atomic% Ar. With such a structure, the stress generated between the substrate 2 and the coating 3 is mitigated, and the hardness of the coating 3 is also increased. As a result, the wear resistance of the coating 3 can be improved.

[0057] The intermediate layer 4 may also contain more than 65 atomic% Ti and more than 1 atomic% Ar. With such a structure, the stress generated between the substrate 2 and the coating 3 can be mitigated, and the hardness of the coating 3 can be further improved. As a result, the wear resistance of the cutting tool 1 is improved.

[0058] The intermediate layer 4 having the above structure can be obtained, for example, by the following manufacturing method.

[0059] (Manufacturing method of the intermediate layer)

[0060] In 8×10 -3 Pa or higher and 1×10 -4The substrate is heated in a reduced-pressure environment of Pa or lower so that the surface temperature is 500°C or higher and 600°C or lower. Next, argon is introduced as an atmospheric gas, and the pressure is maintained at 3.0 Pa. Next, the bias voltage is set to -400 V, and an argon bombardment treatment (pre-argon bombardment treatment) is performed for 11 minutes. Next, the pressure is reduced to 0.1 Pa, an arc current of 100 A or more and 180 A or less is applied to the Ti metal evaporation source, the treatment is performed for 0.5 minutes or more and 1.0 minute or less, and a Ti-containing layer as an intermediate layer is formed on the surface of the substrate (Ti-containing layer film formation treatment). After that, argon is introduced as an atmospheric gas, the pressure is maintained at 3.0 Pa or more and 4.0 Pa or less, the bias voltage is set to -200 V, and an argon bombardment treatment (post-argon bombardment treatment) is performed for 0.3 minutes or more and 0.8 minutes or less.

[0061] Next, the Ti-containing layer film formation treatment and the post-argon bombardment treatment are alternately performed, and this is repeated 1 time or more and 20 times or less. When repeated 1 time, an intermediate layer of about 10 nm is formed, and when repeated 20 times, an intermediate layer of about 200 nm is formed.

[0062] <Processing Conditions for Pre-Argon Bombardment Treatment>

[0063] (1) Bias voltage: -400 V

[0064] (2) Pressure: 3 Pa or lower

[0065] (3) Treatment time: 11 minutes

[0066] <Processing Conditions for Ti-Containing Layer Film Formation Treatment>

[0067] (1) Arc current: 100 A or more and 180 A or less

[0068] (2) Bias voltage: -400 V

[0069] (3) Pressure: 0.1 Pa

[0070] (4) Treatment time: 0.5 minutes or more and 1 minute or less

[0071] <Processing Conditions for Post-Argon Bombardment Treatment>

[0072] (1) Bias voltage: -200 V

[0073] (2) Pressure: 3 Pa or more and 4 Pa or less

[0074] (3) Treatment time: 0.3 minutes or more and 0.8 minutes or less

[0075] <Cutting Tool>

[0076] Next, the structure of the cutting tool provided with the above-described insert 1 will be referred to Figure 4 Let me explain. Figure 4 This is a front view showing an example of a cutting tool involved in the implementation method.

[0077] like Figure 4 As shown, the cutting tool 100 according to the embodiment has a blade 1 and a shank 70 for fixing the blade 1.

[0078] The handle 70 is from the first end ( Figure 4 The upper end of the middle) faces the second end ( Figure 4 A rod-shaped component extending from the lower end of the handle. The handle 70 is, for example, made of steel or cast iron. High-toughness steel is particularly preferred for these components.

[0079] The tool holder 70 has a groove 73 at its first end. The groove 73 is the part for mounting the cutting tool 1, and has a seat surface intersecting the rotation direction of the material being cut and a constraint side inclined relative to the seat surface. A threaded hole for screwing into the screw 75, which will be described later, is provided on the seat surface.

[0080] The cutting blade 1 is located in the groove 73 of the tool holder 70 and is mounted to the tool holder 70 by a screw 75. That is, the screw 75 is inserted into the through hole 21 of the cutting blade 1, and the front end of the screw 75 is inserted into the threaded hole formed in the seat surface of the groove 73, so that the threads are screwed together. Thus, the cutting blade 1 is mounted to the tool holder 70 in such a way that the cutting edge portion protrudes outward from the tool holder 70.

[0081] In this embodiment, a cutting tool for so-called turning is illustrated. Examples of turning include internal diameter machining, external diameter machining, and grooving. It should be noted that the cutting tool is not limited to turning. For example, a cutting tool using insert 1 could also be used for milling. Examples of cutting tools for milling include milling cutters such as face milling, front milling, side milling, or grooving milling, or end mills such as single-flute end mills, multi-flute end mills, tapered end mills, or ball end mills.

[0082] Example

[0083] The embodiments of this disclosure are described in detail below. It should be noted that this disclosure is not limited to the embodiments shown below.

[0084] Samples No. 1 to No. 4 were prepared, each having an intermediate layer and a coating layer on a cermet substrate, the cermet having a hard phase containing Ti and a binder phase containing Co and Ni. Sample No. 1 corresponds to an embodiment of this disclosure, having an intermediate layer containing Ti and Ar and a TiAlN-based coating layer. Specifically, Sample No. 1 has a coating layer composed of TiAlNbWSiN. The specific composition of the coating of Sample No. 1 is Ti.46 Al 49 Nb₂W₂Si₁(N). The intermediate layer and coating are manufactured using the method described above. Sample No. 2 corresponds to an embodiment of this disclosure. Sample No. 2 has: an intermediate layer containing Ti and Al; and a TiAlN-based coating similar to No. 1. Sample No. 3 corresponds to a comparative example. Sample No. 3 has: an intermediate layer containing Al and Cr; and a TiAlN-based coating similar to No. 1. Sample No. 4 corresponds to an example. Sample No. 4 has: an intermediate layer containing Ti and not containing Ar; and a TiAlN-based coating similar to No. 1. For each of Samples No. 1 to No. 3, seven samples with intermediate layer thicknesses of 10 nm, 20 nm, 40 nm, 80 nm, 120 nm, 160 nm, and 200 nm were prepared. In addition, for Sample No. 4, one sample with an intermediate layer thickness of 40 nm was prepared. The coating thickness of each of Samples No. 1 to No. 4 is 3 μm.

[0085] <Hardness Measurement>

[0086] For samples No. 1 to No. 4, the measurement range was defined as the depth from the surface of the coating to a depth of 10% to less than 20% of the coating thickness. The hardness was measured (nanoindentation test) with an indenter load of 50 mN. The measurement was performed using a micro-indentation hardness tester "ENT-1100b / a" (manufactured by Elionix Corporation).

[0087] Specifically, after the indenter comes into contact with the coating surface, a load-displacement curve is obtained by measuring the displacement of the indenter (change in indentation depth) as the load changes through a process of applying load, maintaining maximum load, and releasing load. Furthermore, the hardness is calculated based on the obtained load-displacement curve. This series of measurements is performed 15 times each, and the average value of the hardness measurements from the 15 measurements is calculated.

[0088] Figure 5 It is a graph representing the results of hardness testing. Figure 5 The graph shown has the horizontal axis representing the intermediate layer thickness (nm) and the vertical axis representing the coating hardness (GPa). Figure 5 The data shown in the middle quadrilateral indicates the hardness of the coating of sample No. 1. Figure 5 The data shown by the hollow circles represents the hardness of the coating of sample No. 2. Figure 5 The data shown by the triangle represents the hardness of the coating on sample No. 3. Figure 5 The data indicated by the black circle represents the hardness of the coating on sample No. 4. Figure 5In this context, the data for an intermediate layer thickness of 0 nm represents the hardness measurement results in a sample (hereinafter referred to as "uninserted sample") that does not have an intermediate layer between the substrate and the coating.

[0089] like Figure 5 As shown, it was confirmed that all samples No. 1 to No. 4, when the interlayer thickness was 40 nm, exhibited higher hardness compared to the uninserted sample. In particular, it was confirmed that sample No. 1, as an embodiment of this disclosure, showed significantly higher hardness when the interlayer thickness was 40 nm. Within the range of an interlayer thickness of 20 nm or more and 80 nm or less, the hardness of the coating of sample No. 1 was 33.5 GPa or more.

[0090] On the other hand, it was confirmed that for samples No. 1 to No. 3, the hardness of the coating was lower when the intermediate layer thickness was 200 nm compared to when it was 40 nm. Furthermore, it was confirmed that for samples No. 2 and No. 3, the hardness of the coating was lower when the intermediate layer thickness was 200 nm compared to the uninserted sample.

[0091] <Residual Stress Measurement>

[0092] Figure 6 This is a graph showing the results of measuring the residual stress of the coatings of samples No.1 to No.4. Figure 6 The horizontal axis of the chart shown represents the intermediate layer thickness (nm), and the vertical axis represents the residual compressive stress (GPa).

[0093] It should be noted that in this disclosure, the residual stress is measured at a position at least 1 mm inward (central side) from the cutting edge on the rake face or flank face. X-ray diffraction was used to measure the residual stress. In this disclosure, the 2D method (multiaxial stress measurement method / full Debye ring matching method) was specifically used for X-ray diffraction, but a general X-ray diffraction apparatus can also be used. Furthermore, the X-ray diffraction peak used for residual stress measurement was the peak value of the TiAlN (422) plane where the 2θ value appears between 125° and 135°. The residual stress was calculated using the following conditions: Poisson's ratio of TiAlN = 0.21 and Young's modulus = 600,000 MPa. Additionally, the residual stress was measured under the following conditions: CuKα rays were used as the X-ray source, output = 45 kV, 120 mA. When the residual stress is positive, it is tensile stress; when the residual stress is negative, it is compressive stress. The detailed measurement conditions are as described below.

[0094] <Measurement Conditions>

[0095] X-ray diffraction apparatus: Bruker Japan D8 DISCOVER Plus IμS

[0096] X-ray source: CuKα

[0097] Output: 45kV 120mA

[0098] Collimator diameter: 0.5mmφ

[0099] Diffraction lines were measured: TiAlN(422) plane 2θ≈129.990°

[0100] Measurement method: 2D method (φ angle: 10°, 27.5°, 45°)

[0101] Measurement time: 300 sec / frame

[0102] Measurement location: 1 mm or more inward (central) from the cutting edge.

[0103] Oscillation: θ oscillation (oscillation amplitude: θ = ±2°)

[0104] <Analysis Method>

[0105] The analysis was performed using a 2D method. The following physical property values ​​were used.

[0106] TiAlN(422) surface

[0107] Young's modulus: 600,000 MPa; Poisson's ratio: 0.21

[0108] 2D method: Peak Evaluation: Pearson VII

[0109] Stress model: Biaxial

[0110] exist Figure 6 In the figure, the data for the intermediate layer thickness of 0 nm represents the residual stress of the coating formed directly on the substrate. Additionally, in... Figure 6 The data shown in the middle quadrilateral represents the residual compressive stress results of the coating of sample No. 1. Additionally, in Figure 6 The data shown by the hollow circles represents the residual compressive stress results of the coating in specimen No. 2. Additionally, in Figure 6 The data shown by the triangle represents the residual compressive stress of the coating in specimen No. 3. Additionally, in Figure 6 The data indicated by the black circle represents the residual compressive stress of the coating in specimen No. 4.

[0111] like Figure 6As shown, it was confirmed that the residual compressive stress of the coating decreased with increasing intermediate layer thickness, regardless of the composition of the intermediate layer. In particular, it was found that the residual compressive stress of the coating of sample No. 1, which has an intermediate layer containing Ti and Ar, was significantly reduced compared with that of other samples No. 2 to No. 4. In the range of intermediate layer thickness of 20 nm or more and 80 nm or less, the residual compressive stress of the coating of sample No. 1 was 1.45 GPa or less, specifically 1.4 GPa or less.

[0112] <Determination of Binding Strength>

[0113] For specimens No. 1 to No. 4, the adhesion strength was determined based on a scratch test. The scratch test was conducted using a diamond indenter with a front end shape of 200 μm (radius of curvature), under conditions of a scratching speed of 10 mm / min and an applied load speed of 100 N / min. In the scratch test, the load at which peeling occurred (peel load) was used as the adhesion strength for evaluation. In the scratch test, a higher critical load indicates less likely peeling, i.e., a higher adhesion strength. Figure 7 It is a graph representing the results of the bonding strength measurement. Figure 7 The horizontal axis of the chart shown represents the intermediate layer thickness (nm), and the vertical axis represents the peel load (N). Figure 7 In the figure, the data for the intermediate layer thickness of 0 nm represents the measurement results of the adhesion of the coating in the uninserted sample.

[0114] like Figure 7 As shown, it was confirmed that samples No. 1, No. 2, and No. 4, when the interlayer thickness was 40 nm, exhibited improved adhesion compared to the uninserted sample. In particular, sample No. 1, as an embodiment of this disclosure, showed a significant improvement in adhesion compared to samples No. 2 to No. 4 when the interlayer thickness was 40 nm. Within the range of an interlayer thickness of 20 nm or more and 80 nm or less, the adhesion of sample No. 1 was 110 N or more.

[0115] On the other hand, it was confirmed that for samples No. 1 and No. 2, the adhesion was reduced when the intermediate layer was 200 nm compared to when it was 40 nm. Furthermore, it was confirmed that for sample No. 3, the adhesion of the coating did not change significantly regardless of the thickness of the intermediate layer.

[0116] Figure 8 This is a table summarizing the results of the hardness, stress, and bonding strength measurements described above. Figure 8 In the figure, the hardness, stress, and bonding strength of each sample No.1 to No.3 are shown as percentages when the hardness, stress, and bonding strength of the uninserted sample are all 100%.

[0117] like Figure 8 As shown, when the intermediate layer thickness of Sample No.1, which is an example of the present disclosure, is set to 40 nm, the improvement in hardness and bonding force is remarkable compared with the non-inserted product and Sample No.2 and No.3. In addition, when the intermediate layer thickness of Sample No.1 is set to 40 nm, it exhibits a remarkable stress relaxation effect compared with the non-inserted product, and this effect is also significant even when compared with Sample No.2 and No.3.

[0118] From the above results, it is understood that Sample No.1 having the intermediate layer containing Ti and Ar exhibits excellent comprehensive performance in terms of hardness improvement, stress relaxation, and bonding force improvement when the thickness of the intermediate layer is 40 nm.

[0119] <EDX mapping analysis>

[0120] Elemental analysis based on EDX analysis was performed on Sample No.1. The analysis conditions are as follows.

[0121] (1) Sample pretreatment: Thinning by FIB method (μ-sampling method)

[0122] (2) Elemental analysis (mapping analysis)

[0123] (3) Scanning transmission electron microscope: JEM-ARM200F manufactured by JEOL Ltd.

[0124] (4) Accelerating voltage: 200 kV

[0125] (5) Irradiation current: approximately 7.5 nA

[0126] (6) Elemental analyzer: JED-2300T

[0127] (7) Live time: 60.0 sec

[0128] (8) Energy range: 0 keV or more and 40 keV or less

[0129] Figure 9 is a diagram showing the Ti element mapping image in the intermediate layer of Sample No.1. In addition, Figure 10 is a diagram showing the Ar element mapping image in the intermediate layer of Sample No.1.

[0130] According to Figure 9 and Figure 10 the mapping images shown, it is clearly understood that the intermediate layer of Sample No.1 contains Ti and Ar. In addition, from the Ar mapping image shown in Figure 10 it is clearly understood that the intermediate layer of Sample No.1 has a plurality of Ar-rich regions distributed in an island shape. In addition, as shown in Figure 10As shown, compared to the region on the coating side of the intermediate layer in the thickness direction, there are more Ar-enriched regions in the region on the substrate side of the intermediate layer than the region on the center of the intermediate layer.

[0131] Figure 11 It is Figure 10 The table shows the elemental structure ratios at measurement points P1 to P4, expressed in atomic percent. It should be noted that measurement points P1 and P3 correspond to Ar-enriched regions, while measurement points P2 and P4 correspond to regions outside the Ar-enriched regions in the intermediate layer.

[0132] like Figure 11 As shown, the Ar concentration at measurement points P1 and P3 in the Ar enrichment region is 5 atomic percent. In contrast, the Ar concentration at measurement points P2 and P4 outside the Ar enrichment region is 1 atomic percent. Based on this result, it can be concluded that the Ar enrichment region is a region in the intermediate layer containing at least 3 atomic percent, specifically more than 1 atomic percent, of Ar.

[0133] In addition, according to Figure 11 The results confirmed that, in addition to Ti and Ar, the intermediate layer of sample No. 1 also contained N, Al, Nb, Mo, and W. W was detected at measurement point P2 outside the Ar enrichment region, but not at measurement points P1 and P3 in the Ar enrichment region.

[0134] In addition, according to Figure 11 The results show that the intermediate layer of sample No.1 contains at least 65 atomic% Ti and at least 1 atomic% Ar.

[0135] Wear Test

[0136] Wear tests were conducted on specimens No. 1 to No. 4 (for specimens No. 1 to No. 3, the interlayer thickness was 10 nm, 20 nm, 40 nm, 80 nm, 120 nm, 160 nm, and 200 nm; for specimen No. 4, the interlayer thickness was 40 nm) and specimens without interlayer insertion. The wear tests were performed using a type of cermet material for machining (model: CNMG120408PQ) under the following conditions.

[0137] (1) Cutting method: Wet continuous machining using Φ200 round material.

[0138] (2) Material being cut: SCM435

[0139] (3) Feed f: 0.20 mm / rev

[0140] (4) Cut-in AP: 1.0mm

[0141] (5) Evaluation method: The wear on the side and back face (tool tip wear) after 60 minutes of machining was measured under a microscope.

[0142] Figure 12 It is a graph representing the results of a wear test. Figure 12 The horizontal axis of the graph shows the intermediate layer thickness (nm), and the vertical axis shows the ratio of the tip wear of the uninserted specimen to the tip wear of the specimens with each intermediate layer thickness (the wear resistance ratio). Specifically, the wear resistance ratio is the tip wear of the uninserted specimen / the tip wear of each specimen.

[0143] like Figure 12 As shown, among samples No. 1 to No. 3, in the range where the thickness of the intermediate layer is 10 nm or more and 80 nm or less, the wear amount is reduced compared to the uninserted sample without an intermediate layer. Based on this result, it can be concluded that samples No. 1 to No. 3 exhibit higher wear resistance compared to the uninserted sample in the range where the thickness of the intermediate layer is 10 nm or more and 80 nm or less. Furthermore, it can be seen that among samples No. 1 to No. 3, sample No. 1 exhibits particularly high wear resistance.

[0144] As described above, the blade involved in the embodiment (blade 1, for example) has a substrate (substrate 2, for example) and a coating (coating 3, for example) applied to the surface of the substrate. The substrate is made of cermet. The coating is made of Ti. 1-a-b-c-d Al a M b W c Si d (C x N 1-x The substrate is composed of (wherein, the metal element M is selected from one or more metal elements chosen from Nb, Mo, Ta, Hf, and Y, and 0.40≤a≤0.55, 0.01≤b≤0.1, 0.01≤c≤0.1, 0.01≤d≤0.05, and 0≤x≤1). Furthermore, one embodiment of the blade disclosed herein has an intermediate layer containing Ti disposed between the substrate and the coating (as an example, intermediate layer 4). The average thickness of the intermediate layer is 20 nm or more and 80 nm or less.

[0145] Therefore, the blade according to the embodiment can improve wear resistance.

[0146] It should be noted that, Figure 1 The shape of the blade 1 shown is merely an example and does not limit the shape of the blades disclosed herein. The blades of this disclosure may also have, for example, a rod-shaped body having a rotation axis extending from a first end to a second end; a cutting edge located at the first end of the body; and a groove extending helically from the cutting edge toward the second end of the body.

[0147] Further effects and variations can be readily derived by those skilled in the art. Therefore, the broader scope of this disclosure is not limited to the specific details and representative embodiments described above. Thus, various modifications can be made without departing from the spirit or scope of the overall inventive concept as defined by the technical solutions and their equivalents.

[0148] Explanation of reference numerals in the attached figures

[0149] 1 blade

[0150] 2 matrix

[0151] 3 coatings

[0152] 4 intermediate layers

[0153] 21 through holes

[0154] 41Ar enrichment region

[0155] 70 knife handle

[0156] 73 grooves

[0157] 75 screws

[0158] 100 cutting tools.

Claims

1. A blade, wherein, The blade has a base and a coating applied to the surface of the base. The matrix is ​​composed of metal ceramics. The coating is made of Ti 1-a-b-c-d Al a M b W c Si d (C) x N 1-x It is composed of, wherein the metallic element M is selected from one or more metallic elements from Nb, Mo, Ta, Hf, and Y, and 0.40≤a≤0.55, 0.01≤b≤0.1, 0.01≤c≤0.1, 0.01≤d≤0.05, and 0≤x≤1. An intermediate layer containing Ti is disposed between the substrate and the coating. The average thickness of the intermediate layer is above 20 nm and below 80 nm. The intermediate layer contains more than 65 atomic% Ti and more than 1 atomic% Ar.

2. The blade according to claim 1, wherein, The coating has a hardness of 33.5 GPa or higher and a residual compressive stress of 1.4 GPa or lower.

3. The blade according to claim 1 or 2, wherein, The adhesion strength of the coating is greater than 110N under a peel load in a scratch test.

4. A cutting tool, wherein, The cutting tool has: A handle extending from a first end toward a second end, and having a groove on the side of the first end; and The blade according to any one of claims 1 to 3, located in the groove.