A photocatalyst capable of inhibiting the generation of N2O by-product in a photocatalytic elimination of NOX reaction and a preparation method thereof

By preparing anatase titanium dioxide nanosheets rich in oxygen vacancies, the problems of high cost of nitrogen oxide and soot particle degradation and N2O byproduct generation in existing technologies have been solved, achieving efficient pollutant degradation and compliance with emission standards.

CN118142509BActive Publication Date: 2026-11-10QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410340304.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-25
Publication Date
2026-11-10
Estimated Expiration
2044-03-25

AI Technical Summary

Technical Problem

Existing technologies for degrading nitrogen oxides and particulate matter in motor vehicle exhaust are costly and often generate harmful byproducts such as N2O, making it difficult to meet increasingly stringent emission standards.

Method used

A reduction method was used to treat titanium dioxide nanosheets to generate oxygen vacancy defects, thus preparing anatase titanium dioxide nanosheets rich in oxygen vacancies. These nanosheets were then used to simultaneously degrade nitrogen oxides and carbon soot particles, and to suppress the formation of N2O byproducts.

Benefits of technology

It effectively inhibits the formation of N2O, improves the degradation efficiency of NOx and soot particles, reduces costs, and meets stringent emission standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118142509B_ABST
    Figure CN118142509B_ABST
Patent Text Reader

Abstract

This invention relates to a method for inhibiting photocatalytic elimination of NO X This invention relates to a photocatalyst for the generation of N2O byproducts in a reaction and its preparation method, belonging to the field of photocatalysis technology. The invention uses titanium dioxide nanosheets as the raw material, removing some of the lattice oxygen through a reduction method to generate oxygen vacancy defects, thus obtaining anatase-type titanium dioxide nanosheets rich in oxygen vacancies. This invention simultaneously degrades nitrogen oxides and particulate matter through photocatalysis. The lattice oxygen vacancy defects effectively inhibit N2O generation, especially when the mass ratio of sodium borohydride to titanium dioxide nanosheets is 45:100, the inhibition effect on N2O is most significant, with zero N2O generation observed at reaction times of 30 minutes, 60 minutes, and 120 minutes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalysis technology and relates to a method for inhibiting the photocatalytic elimination of NO. X Photocatalyst for the generation of N2O byproducts in the reaction and its preparation method. Background Technology

[0002] Carbon particulate matter and nitrogen oxides emitted by internal combustion engine vehicles are major contributors to acid rain and photochemical smog, causing harm to both human health and the environment. Studies have shown a significant positive correlation between carbon particulate inhalation and the incidence of cardiovascular and respiratory diseases. Furthermore, with increasingly stringent emission standards for motor vehicles, developing new vehicle exhaust purification technologies to further reduce pollutant concentrations is an urgent issue that needs to be addressed.

[0003] Currently, particulate matter in vehicle exhaust is mainly removed through microfiltration technology, requiring continuous or periodic regeneration of the filters. The degradation of nitrogen oxides, however, requires the use of precious metal catalysts, such as platinum. These methods are not only energy-intensive and costly, but also face significant challenges in further improving their catalytic performance in the face of increasingly stringent emission standards. Photocatalysts are an emerging, green, and environmentally friendly technology that can oxidize and reduce nitrogen oxides and particulate matter at room temperature using only light irradiation. The products of photocatalytic degradation of particulate matter are CO2 and CO. Nitrogen oxides can be oxidized to nitrates or reduced to nitrogen gas. Previous research results indicate that anatase titanium dioxide is an effective photocatalyst for degrading nitrogen oxides and particulate matter. Titanium dioxide can reduce NO to N2 and oxidize particulate matter to CO at room temperature using only light irradiation. x However, harmful gas N2O often appears as a byproduct. Furthermore, N2O has a strong greenhouse effect. The inventors used titanium dioxide nanosheets as raw materials and employed a strong reducing agent to partially reduce its lattice oxygen, thereby generating highly active oxygen vacancies. These oxygen vacancies can effectively capture photogenerated charges, reduce their recombination rate, enhance the photocatalytic activity of titanium dioxide, and effectively inhibit the formation of N2O byproducts.

[0004] The inhibition of N2O byproducts can be achieved by preparing and modifying single-component photocatalysts. The preparation method is simple, low-cost, and has good application prospects. Summary of the Invention

[0005] To address the high cost and frequent N2O byproduct formation associated with the removal of nitrogen oxides and particulate matter, the main pollutants in automobile exhaust, this invention provides a method for inhibiting the photocatalytic elimination of NO. XPhotocatalyst for N2O byproduct formation and its preparation method. This invention utilizes titanium dioxide nanosheets as a single photocatalyst to simultaneously degrade nitrogen oxides and particulate matter pollutants via photocatalysis. To improve the photocatalytic activity of titanium dioxide nanosheets, especially to suppress the formation of the byproduct N2O, titanium dioxide nanosheets were selected as the raw material. A reduction method was used to remove some of the lattice oxygen, generating oxygen vacancy defects. These defective titanium dioxide nanosheets were then used in the simultaneous elimination reaction of nitrogen oxides and particulate matter. Results show that lattice oxygen vacancy defects can effectively suppress N2O formation and reduce NO formation. X The degradation efficiency of carbon soot particles is improved. The technical solution of this method is as follows: A method to inhibit photocatalytic elimination of NO X The preparation method of the photocatalyst for the formation of N2O byproducts in the reaction is as follows: (1) Slowly add hydrofluoric acid to tetrabutyl titanate and continuously stir magnetically for 2-4 hours until the solution forms a gel-like solution. Transfer the mixture into the reaction vessel. (2) The reaction vessel was placed in an oven for high-temperature crystallization, with the temperature controlled at 150 ℃~210 ℃ and the time controlled at 10~40 hours. After naturally cooling to room temperature, it was washed with water and ethanol in sequence, centrifuged, and then dried in a vacuum drying oven at 80 ℃ for 5~24 hours to obtain titanium dioxide nanosheets A. (3) Add titanium dioxide nanosheets A to anhydrous ethanol, stir continuously for 30 min, add sodium borohydride as a reducing agent, stir continuously until homogeneous, transfer the mixture to a muffle furnace and calcine at 500 °C for 3-5 hours, then cool to room temperature; (4) Remove unreacted reducing agent by acid washing of the calcined sample: Add the sample obtained in step (3) to a 1 mol / L hydrochloric acid solution, stir magnetically for 6 hours, filter and wash with water until neutral, and dry at 60 °C to obtain anatase titanium dioxide nanosheets rich in oxygen vacancies. Preferably, in step (1), the volume ratio of hydrofluoric acid to tetrabutyl titanate is 3:25.

[0006] Preferably, the crystallization temperature in step (2) is 180 °C, and the crystallization time is 24 hours; The centrifugation speed was 10,000 rpm, the centrifugation time was 5 min, and the number of centrifugations was 10.

[0007] Preferably, in step (3), the mass-to-volume ratio of titanium dioxide nanosheets A to anhydrous ethanol is 0.3:25, g / mL; in step (3), the mass ratio of reducing agent sodium borohydride to titanium dioxide nanosheets A is 1~100:100; more preferably, the mass ratio of sodium borohydride to titanium dioxide nanosheets A is 5~60:100; more preferably, the mass ratio of sodium borohydride to titanium dioxide nanosheets A is 45:100.

[0008] Preferably, the ratio of the sample obtained in step (3) to the hydrochloric acid solution in step (4) is 0.1:20, g / mL.

[0009] Compared with the prior art, the present invention has the following advantages: The oxygen-vacancy-rich anatase titanium dioxide nanosheets provided by this invention are used in the photocatalytic simultaneous elimination reaction of nitrogen oxides and soot particles. Compared with existing titanium dioxide nanosheets, they exhibit varying degrees of inhibition on N2O formation. The inhibition effect on N2O is most significant when the mass ratio of sodium borohydride to titanium dioxide nanosheets is 45:100, with zero N2O generation observed at reaction times of 30 minutes, 60 minutes, and 120 minutes. Attached Figure Description

[0010] Figure 1 The XRD pattern of the titanium dioxide nanosheet photocatalyst is shown. Figure 2 Here are SEM images of titanium dioxide nanosheet photocatalysts, where... 2a and 2b are both scanning electron microscope images of pristine TiO2; 2c and 2d are both scanning electron microscope images of anatase titanium dioxide nanosheets rich in oxygen vacancies, produced by using sodium borohydride to titanium dioxide nanosheets in a mass ratio of 5:100. Images 2e and 2f are both scanning electron microscope (SEM) images of oxygen-vacancy-rich anatase titanium dioxide nanosheets made with sodium borohydride and titanium dioxide nanosheets in a mass ratio of 15:100. Detailed Implementation

[0011] The following examples are merely illustrative of embodiments of the present invention and do not constitute any limitation on the invention. Those skilled in the art will understand that modifications made without departing from the spirit and concept of the invention fall within the protection scope of the present invention. Unless otherwise specified, the reagents and instruments used in the following examples are commercially available products.

[0012] Example 1 (1) Slowly add 3 ml of HF to 25 ml of tetrabutyl titanate and stir magnetically for 2 hours until the solution forms a gel-like solution. Transfer the mixture into the reaction vessel.

[0013] (2) Place the reactor in an oven for high-temperature crystallization at 180°C. o Heated at C for 24 hours. After naturally cooling to room temperature, washed with deionized water and ethanol respectively, and centrifuged 10 times at 10,000 rpm to remove residual organic matter and fluoride ions. The obtained sample was then dried in a vacuum oven at 80°C. o Titanium dioxide nanosheets (TNS) were obtained by drying at C for 5 hours.

[0014] (3) Mix 0.3 g of titanium dioxide nanosheets with 25 ml of ethanol, stir on a magnetic stirrer for 30 min, add sodium borohydride (mass ratio of sodium borohydride to titanium dioxide nanosheets is 45:100), and stir magnetically for 1 hour. Transfer the mixture to a muffle furnace at 500 °C. o Roast at C for 3 hours, then cool to room temperature.

[0015] (4) Add the calcined substance to 60 ml of hydrochloric acid (1 mol / L), stir magnetically for 6 hours, filter and wash with water until neutral, and dry in a drying oven at 60°C. o Drying at C yields oxygen-vacancy-rich photocatalyst titanium dioxide nanosheets.

[0016] Example 2 (1) Slowly add 3 ml of HF to 25 ml of tetrabutyl titanate and stir magnetically for 4 hours until the solution forms a gel-like solution. Then put the mixture into the reaction vessel.

[0017] (2) Place the reactor in an oven for high-temperature crystallization at 200°C. o Heated at C for 18 hours. After naturally cooling to room temperature, washed with deionized water and ethanol respectively, and centrifuged 10 times at 10,000 rpm to remove residual organic matter and fluoride ions. The obtained sample was then dried in a vacuum oven at 80°C. o Titanium dioxide nanosheets were obtained by drying at C for 6 hours.

[0018] (3) Mix 0.3 g of titanium dioxide nanosheets with 25 ml of ethanol, stir on a magnetic stirrer for 30 min, add sodium borohydride (sodium borohydride to titanium dioxide nanosheets mass ratio of 30:100), and stir magnetically for 1 hour. Transfer the mixture to a muffle furnace at 500 °C. o Roast at C for 3 hours, then cool to room temperature.

[0019] (4) Add the calcined substance to 60 ml of hydrochloric acid (1 mol / L), stir magnetically for 6 hours, filter and wash with water until neutral, and dry in a drying oven at 60°C. o Drying at C yields anatase titanium dioxide nanosheets, a photocatalyst rich in oxygen vacancies.

[0020] Example 3 (1) Slowly add 3 ml of HF to 25 ml of tetrabutyl titanate and stir magnetically for 2 hours until the solution forms a gel-like solution. Then put the mixture into the reaction vessel.

[0021] (2) Place the reactor in an oven for high-temperature crystallization at 160°C. o Heated at C for 32 hours. After naturally cooling to room temperature, washed with deionized water and ethanol respectively, and centrifuged 10 times at 10,000 rpm to remove residual organic matter and fluoride ions. The obtained sample was then dried in a vacuum oven at 80°C. o Titanium dioxide nanosheets were obtained by drying at C for 5 hours.

[0022] (3) Mix 0.3 g of titanium dioxide nanosheets with 25 ml of ethanol, stir on a magnetic stirrer for 30 min, add sodium borohydride (sodium borohydride to titanium dioxide nanosheets mass ratio of 15:100), and stir magnetically for 1 hour. Transfer the mixture to a muffle furnace at 500 °C. o Roast at C for 3 hours, then cool to room temperature.

[0023] (4) Add the calcined substance to 60 ml of hydrochloric acid (1 mol / L), stir magnetically for 6 hours, filter and wash with water until neutral, and dry in a drying oven at 60°C. o Drying at C yields anatase titanium dioxide nanosheets, a photocatalyst rich in oxygen vacancies.

[0024] Example 4 (1) Slowly add 3 ml of HF to 25 ml of tetrabutyl titanate and stir magnetically for 2 hours until the solution forms a gel-like solution. Then put the mixture into the reaction vessel.

[0025] (2) Place the reactor in an oven for high-temperature crystallization at 180°C. o Heated at C for 40 hours. After naturally cooling to room temperature, washed with deionized water and ethanol respectively, and centrifuged 10 times at 10,000 rpm to remove residual organic matter and fluoride ions. The obtained sample was then dried in a vacuum oven at 80°C. o Titanium dioxide nanosheets were obtained by drying at C for 5 hours.

[0026] (3) Mix 0.3 g of titanium dioxide nanosheets with 25 ml of ethanol, stir on a magnetic stirrer for 30 min, add sodium borohydride (sodium borohydride to titanium dioxide nanosheets mass ratio of 10:100), and stir magnetically for 1 hour. Transfer the mixture to a muffle furnace at 500 °C. o Roast at C for 3 hours, then cool to room temperature.

[0027] (4) Add the calcined substance to 60 ml of hydrochloric acid (1 mol / L), stir magnetically for 6 hours, filter and wash with water until neutral, and dry in a drying oven at 60°C.o Drying at C yields anatase titanium dioxide nanosheets, a photocatalyst rich in oxygen vacancies.

[0028] Example 5 (1) Slowly add 3 ml of HF to 25 ml of tetrabutyl titanate and stir magnetically for 2 hours until the solution forms a gel-like solution. Then put the mixture into the reaction vessel.

[0029] (2) Place the reactor in an oven for high-temperature crystallization at 200°C. o Heated at C for 24 hours. After naturally cooling to room temperature, washed with deionized water and ethanol respectively, and centrifuged 10 times at 10,000 rpm to remove residual organic matter and fluoride ions. The obtained sample was then dried in a vacuum oven at 80°C. o Titanium dioxide nanosheets were obtained by drying at C for 7 hours.

[0030] (3) Mix 0.3 g of titanium dioxide nanosheets with 25 ml of ethanol, stir on a magnetic stirrer for 30 min, add sodium borohydride (sodium borohydride to titanium dioxide nanosheets mass ratio of 5:100), and stir magnetically for 1 hour. Transfer the mixture to a muffle furnace at 500 °C. o Roast at C for 3 hours, then cool to room temperature.

[0031] (4) Add the calcined substance to 60 ml of hydrochloric acid (1 mol / L), stir magnetically for 6 hours, filter and wash with water until neutral, and dry in a drying oven at 60°C. o Drying at C yields anatase titanium dioxide nanosheets, a photocatalyst rich in oxygen vacancies.

[0032] Comparative Example (1) Slowly add 3 ml of HF to 25 ml of titanium oxysulfate and stir magnetically for 2 hours until the solution forms a gel-like solution. Then put the mixture into the reaction vessel.

[0033] (2) Place the reactor in an oven for high-temperature crystallization at 160°C. o Heated at C for 24 hours. After naturally cooling to room temperature, washed with deionized water and ethanol respectively, and centrifuged 10 times at 10,000 rpm to remove residual organic matter and fluoride ions. The obtained sample was then dried in a vacuum oven at 80°C. o Titanium dioxide nanosheets (TNS) were obtained by drying at C for 5 hours.

[0034] Experimental Example 1: This experiment investigated the NO content of the oxygen-vacancy titanium dioxide nanosheet photocatalysts in Examples 1-5. XThe photocatalytic performance of the synergistic removal reaction with soot particles was tested. In a typical sample preparation process, 5 mg of carbon black (U-carbon) was dispersed in isopropanol and then uniformly dropped onto a glass plate (300 mm * 50 mm) to form a carbon black layer. Subsequently, 50 mg of white TiO2 nanosheets or oxygen-vacancy TiO2 nanosheet photocatalyst was deposited on the soot layer by diffusion and evaporation of the 2-propanol suspension. The soot-photocatalyst coated glass plate was dried overnight at 60 °C. The sample plate was sealed in a reactor and irradiated from above with ultraviolet light at a wavelength of 350 nm at room temperature with a light intensity of 1.1 mW / cm². 2 500 ppm NO (5% NO and 95% He) and 5% O2, along with carrier gas N2 (99.999%), were introduced into the reactor. The total flow rate of the reaction gas was controlled at 150 mL / min using a gas flow meter. The gas flow was maintained for 10 min, after which the inlet and outlet were closed, and the reactor was sealed. The UV lamp was then turned on to initiate the photoreaction. The gaseous products after the reaction were automatically detected using a UV gas detector (NO and NO2 were detected using a CUBIC-RUIYI GASBOARD 3000UV; CO and CO2 were detected using a CUBIC-RUIYI GASBOARD 3000PLUS). N2O was detected using a GEOTECH G200 analyzer. Nitrogen selectivity was calculated based on nitrogen atom conservation. Solid products were measured using Fourier transform infrared spectroscopy. As described above, each sample was continuously tested for 30 min, 60 min, and 120 min, for a total of 210 min.

[0035] Table 1. Evaluation Results of Photocatalytic Reaction Performance

[0036] The results in Table 1 show that the oxygen-vacancy titanium dioxide nanosheets provided by this invention have stronger photocatalytic activity than the original sample, and also significantly inhibit the formation of N2O.

[0037] Experimental Example 2: The XRD pattern of the oxygen-vacancy titanium dioxide nanosheet photocatalyst prepared in this invention is shown below. Figure 1 As shown, from Figure 1 As can be seen, the original nanosheets and the oxygen-vacancy nanosheets have the same crystal form, both being anatase titanium dioxide (JCPDS card number: 21-1272). The SEM image of the oxygen-vacancy titanium dioxide nanosheet photocatalyst prepared in this invention is shown below. Figure 2As shown, 2a and 2b are scanning electron microscope (SEM) images of pristine TiO2, 2c and 2d are SEM images of anatase titanium dioxide nanosheets rich in oxygen vacancies after treatment with sodium borohydride to titanium dioxide nanosheets at a mass ratio of 5:100, and 2e and 2f are SEM images of anatase titanium dioxide nanosheets rich in oxygen vacancies after treatment with sodium borohydride to titanium dioxide nanosheets at a mass ratio of 15:100.

[0038] from Figure 2 It can be seen that both the original titanium dioxide and the titanium dioxide reduced by the reducing agent have the morphology of nanosheets. The original nanosheets are larger in size, while the nanosheets after reduction treatment are significantly smaller in size.

[0039] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments, or make equivalent substitutions for some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to depart from the spirit and scope of the technical solutions claimed by the present invention.

Claims

1. A photocatalyst for the synergistic catalytic elimination of NO X Its application in the reaction of N2O and soot particles is characterized by, The application conditions are as follows: The sample plate sealed in the reactor was irradiated from above at room temperature using ultraviolet light with a wavelength of 350 nm; the reaction gases NO and O2 and the carrier gas N2 were introduced into the reactor. The sample plate was prepared as follows: Carbon black (U-carbon) was dispersed in isopropanol and then uniformly dropped onto a glass plate to form a carbon black layer. Subsequently, the photocatalyst was deposited on the soot layer by diffusion and evaporation of the 2-propanol suspension, and the glass plate was dried overnight. The preparation method of the photocatalyst includes the following steps: (1) Slowly add hydrofluoric acid to tetrabutyl titanate and continuously stir magnetically for 2-4 hours until the solution forms a gel-like solution. Transfer the mixture into the reaction vessel. (2) The reaction vessel was placed in an oven for high-temperature crystallization, with the temperature controlled at 150 ℃~210 ℃ and the time controlled at 10~40 hours. After naturally cooling to room temperature, it was washed with water and ethanol in sequence, centrifuged, and then dried in a vacuum drying oven at 80 ℃ for 5~24 hours to obtain titanium dioxide nanosheets A. (3) Add titanium dioxide nanosheets A to anhydrous ethanol, stir continuously for 30 min, add sodium borohydride as a reducing agent, stir continuously until homogeneous, transfer the mixture to a muffle furnace and calcine at 500 °C for 3-5 hours, then cool to room temperature; (4) Remove unreacted reducing agent by acid washing of the calcined sample: Add the sample obtained in step (3) to a 1 mol / L hydrochloric acid solution, stir magnetically for 6 hours, filter and wash with water until neutral, dry at 60 °C to obtain anatase titanium dioxide nanosheets rich in oxygen vacancies. In step (1), the volume ratio of hydrofluoric acid to tetrabutyl titanate is 3:

25. In step (3), the mass-to-volume ratio of titanium dioxide nanosheets A to anhydrous ethanol is 0.3:25, g / mL; in step (3), the mass ratio of reducing agent sodium borohydride to titanium dioxide nanosheets A is 1~100:

100.

2. The application according to claim 1, characterized in that, The crystallization temperature in step (2) is 180 °C and the crystallization time is 24 hours.

3. The application according to claim 1, characterized in that, In step (2), the centrifugation speed is 10,000 rpm, the centrifugation time is 5 min, and the number of centrifugations is 10.

4. The application according to claim 1, characterized in that, The mass ratio of sodium borohydride to titanium dioxide nanosheets A is 5~60:

100.

5. The application according to claim 4, characterized in that, The mass ratio of sodium borohydride to titanium dioxide nanosheets A is 45:

100.

6. The application according to claim 1, characterized in that, The ratio of the sample obtained in step (3) to the hydrochloric acid solution in step (4) is 0.1:20 g / mL.

Citation Information

Patent Citations

  • Trivalent titanium ion self-doped titanium dioxide nanosheet catalyst

    CN105664902A

  • Preparation method of defective titanium dioxide / ultrathin carbon nitride / defective titanium dioxide Z-type heterojunction photocatalyst

    CN114345393A