Tungsten wire, sawing wire and tungsten wire for screen printing
By controlling the surface grain width and wire diameter of tungsten or tungsten alloy wires, combined with specific manufacturing processes, the tensile strength of tungsten wires has been improved, solving the problem of insufficient tensile strength of existing tungsten alloy wires and enabling their widespread application in multiple fields.
Patent Information
- Application Number
- CN202410290782.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-19
- Filing Date
- 2021-05-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-05-26
AI Technical Summary
Existing tungsten alloy wires have insufficient tensile strength, making them difficult to utilize effectively in many fields, especially failing to meet industrial requirements in terms of chemical stability and high elastic modulus.
By controlling the surface grain width and wire diameter of tungsten or tungsten alloy wires, the average surface grain width is ensured to be below 98nm and the wire diameter is between 100μm and 225μm. Through specific manufacturing processes such as room temperature wire drawing and electrolytic polishing, the tensile strength is increased to above 3900MPa.
It achieves higher tensile strength than piano wire and is suitable for a variety of industrial applications, including saw wire, screen printing and medical needles.
Smart Images

Figure CN118143267B_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application filed on May 26, 2021, with application number 202180036096.5 and invention title "Tungsten Wire, Saw Wire and Tungsten Wire for Screen Printing". Technical Field
[0002] This invention relates to tungsten wire, saw wire, and tungsten wire for screen printing. Background Technology
[0003] Previously, medical needles with high tensile strength were known to be made from tungsten alloy wires with an increased alloy ratio relative to tungsten (see, for example, Patent Document 1). Patent Document 1 discloses a tungsten alloy wire with a diameter of 0.10 mm and a maximum tensile strength of 4459.0 N / mm². 2 (=MPa).
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-169499 Summary of the Invention
[0007] The problem that the invention aims to solve
[0008] To enable its effective use in various fields beyond medical needles, tungsten wire with higher tensile strength than ever before is required. As a metallic wire, tungsten, with its chemical stability, high elastic modulus, and high melting point, is highly anticipated in industry, compared to piano wire, which boasts the highest strength.
[0009] Therefore, the object of the present invention is to provide tungsten wire, saw wire, and tungsten wire for screen printing that have a higher tensile strength than that of piano wire.
[0010] Methods for solving problems
[0011] One embodiment of the present invention is a tungsten wire formed of tungsten or a tungsten alloy, wherein the average width of the surface grains of the tungsten wire in the direction perpendicular to the wire axis is 98 nm or less, the tensile strength of the tungsten wire is 3900 MPa or more, and the wire diameter is greater than 100 μm and less than 225 μm.
[0012] Furthermore, in one embodiment of the present invention, the tungsten wire is a tungsten wire formed of tungsten or a tungsten alloy, wherein the average width of the surface grains in the direction perpendicular to the wire axis is 98 nm or less, the tensile strength of the tungsten wire is 3900 MPa or more, and the wire diameter is 18 μm or more and 225 μm or less. When the tensile strength is set to T [MPa] and the wire diameter is set to D [mm], T ≥ 4758 × D2 -7258.3×D+5275.5 holds true.
[0013] One embodiment of the present invention provides a saw wire comprising the aforementioned tungsten wire.
[0014] One aspect of the present invention provides a tungsten wire for screen printing comprising the aforementioned tungsten wire.
[0015] Invention Effects
[0016] According to the present invention, it is possible to provide tungsten wire, etc., with a tensile strength higher than that of typical piano wire. Attached Figure Description
[0017] Figure 1 This is a schematic perspective view of the tungsten wire in the embodiment.
[0018] Figure 2A This is a magnified view of the surface of the tungsten wire from Example 1.
[0019] Figure 2B This is a magnified view of the surface of the tungsten wire in Example 2.
[0020] Figure 2C This is a magnified view of the surface of the tungsten wire in Example 3.
[0021] Figure 2D This is a magnified view of the surface of the tungsten wire in Example 4.
[0022] Figure 2E This is a magnified view of the surface of the tungsten wire in Example 5.
[0023] Figure 3 This is a graph showing the relationship between the average width of surface grains and tensile strength.
[0024] Figure 4 It is a graph showing the relationship between wire diameter and tensile strength.
[0025] Figure 5 This is a flowchart illustrating a method for manufacturing tungsten wire according to an embodiment.
[0026] Figure 6 This is a perspective view showing the cutting device according to the embodiment.
[0027] Figure 7 This is a perspective view of the screen used in the embodiment. Detailed Implementation
[0028] Hereinafter, tungsten wire, saw wire, and tungsten wire for screen printing according to embodiments of the present invention will be described in detail with reference to the accompanying drawings. Furthermore, the embodiments described below represent specific examples of the present invention. Therefore, the numerical values, shapes, materials, constituent elements, arrangements and connection methods of constituent elements, steps, and order of steps shown in the following embodiments are merely examples and are not intended to limit the scope of the present invention. Therefore, in the constituent elements of the following embodiments, constituent elements not described in the independent claims will be described as optional constituent elements.
[0029] Furthermore, these figures are schematic diagrams and not necessarily strictly representational. Therefore, for example, the scales may not be consistent across figures. Additionally, in each figure, the same symbols are used to label substantially the same components, and repeated descriptions are omitted or simplified.
[0030] Furthermore, in this specification, terms such as vertical or consistent indicating the relationship between elements, terms such as circle or rectangle indicating the shape of elements, and numerical ranges are not merely expressions of a strict meaning, but also imply expressions that include substantially equivalent ranges, such as differences of several percentage points.
[0031] (Implementation Method)
[0032] [Tungsten wire]
[0033] First, the structure of the tungsten wire in the embodiment will be explained.
[0034] Figure 1 This is a schematic perspective view of the tungsten wire 10 in this embodiment. Figure 1 The image shows an example of a tungsten wire 10 being wound onto a core material for winding, and further, a portion of the tungsten wire 10 is enlarged and schematically represented.
[0035] The tungsten wire 10 in this embodiment is formed of tungsten (W) or a tungsten alloy. The tungsten content in the tungsten wire 10 is, for example, 99% by weight or more. The tungsten content can be 99.5% by weight or more, 99.9% by weight or more, or 99.99% by weight or more. Furthermore, the tungsten content is the ratio of the weight of tungsten to the weight of the tungsten wire 10. The same applies to the content of other metallic elements such as rhenium (Re) and potassium (K), which will be described later.
[0036] Tungsten alloys, for example, are rhenium-tungsten alloys (ReW alloys). The higher the rhenium content, the higher the tensile strength of the tungsten wire 10. However, if the rhenium content is too high, for example, if the rhenium content exceeds 9% by weight, thinning of the tungsten wire while maintaining a high tensile strength of the tungsten wire 10 will result in wire breakage, making it difficult to draw long strips of wire.
[0037] In this embodiment, the rhenium content in the tungsten wire 10 is 0.1% by weight or more and 1% by weight or less. For example, the rhenium content may also be 0.5% by weight or more.
[0038] Additionally, the tungsten wire 10 may contain unavoidable impurities that are difficult to prevent during manufacturing. Furthermore, the tungsten content may be less than 99% by weight, and the rhenium content may be greater than 1% by weight.
[0039] The diameter of the tungsten wire 10 is 225 μm or less. For example, the diameter of the tungsten wire 10 is greater than 100 μm and less than 225 μm. Alternatively, the diameter of the tungsten wire 10 can also be less than 100 μm. The diameter of the tungsten wire 10 can also be greater than 18 μm and less than 225 μm.
[0040] In this embodiment, the diameter of the tungsten wire 10 is uniform. However, it may not be completely uniform; depending on the location along the spool direction, it may contain a difference of approximately 1% or several percentage points. The tungsten wire 10 is as follows... Figure 1 As shown, for example, the cross-sectional shape of a section orthogonal to the linear axis P is circular. The cross-sectional shape can also be square, rectangular, or elliptical, etc.
[0041] Furthermore, the elastic modulus of the tungsten wire 10 is between 350 GPa and 450 GPa. Here, the elastic modulus refers to the longitudinal elastic modulus. Additionally, the elastic modulus of piano wire is generally in the range of 150 GPa to 250 GPa. That is, the tungsten wire 10 has approximately twice the elastic modulus of piano wire. The phrase "approximately twice the elastic modulus" means that, for the same wire diameter, the flexural capacity of the tungsten wire is approximately half that of the piano wire. Furthermore, the flexural capacity is the amount of flexural deformation when the tungsten wire or piano wire is supported at both ends, and is calculated by approximating each wire as a "beam (crossbeam)". If the flexural capacity is set to be the same, then when the diameter of the piano wire is set to 100%, the diameter of the tungsten wire 10 becomes approximately 84%, which is about 16% thinner. When used as a saw wire, cutting costs can be reduced.
[0042] With an elastic modulus of 350 GPa or higher, the tungsten wire 10 becomes difficult to deform. That is, the tungsten wire 10 becomes difficult to stretch. On the other hand, with an elastic modulus of 450 GPa or lower, even with a high elastic modulus, if the tensile strength (stress) is sufficiently high, the tungsten wire 10 can be deformed due to the increased stretching (strain) in the elastic region. Specifically, the tungsten wire 10 can be bent, and therefore, for example, when used as a saw wire, it can be easily wound onto guide rollers or the like.
[0043] The tungsten wire 10, formed from tungsten or a tungsten alloy, has a tensile strength of 3900 MPa or higher. Furthermore, the tensile strength of the tungsten wire 10 can also be 5000 MPa or higher, or even 5300 MPa or higher. The tensile strength of the tungsten wire 10 has a defined relationship with respect to the rhenium content, wire diameter, and average width of the surface grains in the tungsten wire 10. Therefore, the tensile strength of the tungsten wire 10 can be set to a desired value by appropriately adjusting at least one of the rhenium content, wire diameter, and average width of the surface grains. For example, it is possible to achieve a tungsten wire 10 with a high tensile strength exceeding approximately 5500 MPa. The relationship between tensile strength and various parameters will be explained below.
[0044] [Average width of surface grains]
[0045] First, the relationship between the tensile strength of tungsten wire and the average width of the surface grains is explained.
[0046] The surface grains are tungsten or tungsten alloy grains on the surface of the tungsten wire. In the tungsten wire of this embodiment, the average width of the surface grains in the direction orthogonal to the wire axis P is 98 nm or less. The width of the surface grains in the direction orthogonal to the wire axis P refers to the length of the surface grains along the direction orthogonal to the wire axis P.
[0047] The following explains the relationship between the tensile strength and the width of the surface grains of the multiple tungsten wire samples manufactured by the inventors.
[0048] Figures 2A-2E These are magnified images of the surface of the tungsten wires from Examples 1 to 5. Each image represents a SEM (Scanning Electron Microscope) image of the tungsten wire surface. The areas represented in each image are, for example, as shown below. Figure 1 The area shown corresponds to the rectangular region enclosed by dashed lines on the surface 20 of tungsten wire 10. In each figure, a region of the same concentration (color) represents one grain. The left-right direction of each figure is parallel to the line axis P. The grains extend in elongated strips along the line axis P.
[0049] In each figure, the solid line L drawn near the center is a straight line extending in a direction perpendicular to the line axis P. The average width of the surface grains is calculated by counting the number of grain boundaries (i.e., grain boundaries) along the solid line L within the range shown in each figure. Specifically, the average width of the surface grains is calculated by dividing the length of the solid line L within the counting range by "grain boundary number + 1". Additionally, in each figure, multiple short line segments orthogonal to the solid line L represent grain boundaries.
[0050] The relationship between the average width of surface grains calculated based on the grain boundary number and tensile strength is shown in Table 1.
[0051] Table 1
[0052]
[0053] Furthermore, Examples 1 to 5 shown in Table 1 are 99.5% by weight tungsten wires. The processing rates in Table 1 are for room temperature wire drawing. Details regarding the processing rates are explained below along with the tungsten wire manufacturing method.
[0054] Figure 3 This is a graph showing the relationship between the average width of surface grains and tensile strength. In Figure 3 In the graph, the horizontal axis represents the average width of the surface grains [nm], and the vertical axis represents the tensile strength [MPa]. Furthermore, Figure 3 The values 1 to 8 recorded next to each plot refer to the measurement results of each plot for Examples 1 to 8.
[0055] As shown in Table 1 and Figure 3 As shown, there is a negative correlation between the average width of the surface grains and the tensile strength. That is, the smaller the average width of the surface grains, the higher the tensile strength. In particular, as can be seen from comparing Example 2 and Example 3, even with the same wire diameter of 32 μm and the same tungsten content of 99.5% by weight, different average widths of the surface grains can result in different tensile strengths. Furthermore, the average width of the surface grains can be adjusted by varying the processing rate of the room temperature drawing. Specifically, a higher processing rate of the room temperature drawing results in a smaller average width of the surface grains and thus a higher tensile strength.
[0056] Figure 3 The samples (Examples 6-8) with a wire diameter of 50 μm were also plotted using circular symbols. The relationship between the average width of the surface grains of Examples 6-8 and their tensile strength is shown in Table 2.
[0057] Table 2
[0058]
[0059] Regarding the relationship between the tensile strength and the average width of the surface grains of the samples in Examples 6 to 8, if it is obtained by polynomial approximation, then when the tensile strength is set to T [MPa] and the average width of the surface grains is set to W [nm], the following equation (1) holds.
[0060] (1) T = 0.3088 × W 2 -72.798×W+8516.8
[0061] Furthermore, if the diameter of the tungsten wire is different, the coefficients of equation (1) also change, but the negative correlation between the tensile strength T and the average width W of the surface grains remains unchanged. Moreover, even in cases where the wire diameters are significantly different, such as... Figure 3 As shown, the tensile strength T and the average width W of the surface grains also have a relationship that is approximately within the range of -500 MPa to +200 MPa, with the curve shown in Equation (1) as the reference. That is, regardless of the wire diameter, the tensile strength T and the average width W of the surface grains satisfy the relationship expressed by the inequality in Equation (2) below.
[0062] (2) 0.3088×W 2 -72.798×W+8016.8≤T≤0.3088×W 2 -72.798×W+8716.8
[0063] As described above, by reducing the average width of the surface grains, it is possible to achieve tungsten wires with high tensile strength.
[0064] [Wire Diameter]
[0065] Next, the relationship between the tensile strength and diameter of tungsten wire will be explained.
[0066] Figure 4 This is a graph showing the relationship between wire diameter and tensile strength. In Figure 4 In the figure, the horizontal axis represents the diameter of the tungsten wire [μm], and the vertical axis represents the tensile strength of the tungsten wire [MPa]. Figure 4 The values 1 to 5 and 9 to 11 recorded next to each plot refer to the measurement results of each plot for Examples 1 to 5 and 9 to 11 respectively.
[0067] like Figure 4 As shown, there is a negative correlation between wire diameter and tensile strength. That is, the smaller the wire diameter, the higher the tensile strength, and the larger the wire diameter, the lower the tensile strength.
[0068] In the tungsten wire of this embodiment, when the wire diameter is set to D [mm], the following formula (3) is satisfied.
[0069] (3) 4758×D 2 -7258.3×D+5275.5≤T≤4758×D 2 -7258.3×D+6100
[0070] The quadratic function on the left side of the inequality (3) is... Figure 4 The solid line represents the solid line. Figure 4The solid lines are obtained by polynomial approximation using plots with a processing rate of 70% at room temperature drawing (the five plots shown in the circles). The five plots with the circles correspond to Examples 1, 3-5 shown in Table 1 and Example 9 shown in Table 3.
[0071] Table 3
[0072]
[0073] The quadratic function on the right side of the inequality (3) is... Figure 4 The dashed line represents this. Figure 4 The dotted line is to Figure 4 The line is obtained by moving the solid line parallel to it, and it is a line drawn through the triangle mark corresponding to Example 2 (processing rate of 90% at room temperature drawing). That is, even with the same wire diameter, the tensile strength can be increased by increasing the processing rate of room temperature drawing.
[0074] in addition, Figure 4 The dotted lines in the diagram represent the range of wire diameter and tensile strength relationships disclosed in Patent Document 1 that satisfy conventional requirements. According to this embodiment, by setting the room-temperature drawing rate to 70% or more and adjusting the average width of the surface grains, tungsten wire with higher tensile strength than previously possible can be achieved.
[0075] [Rhenium content]
[0076] Next, the relationship between the rhenium content in the tungsten wire and the wire diameter will be explained.
[0077] Figure 4 The Chinese character is represented by a four-corner symbol. Figure 3 Examples 10 and 11 are shown. As by Figure 4 As demonstrated, even with the same wire diameter, increasing the rhenium content makes it easier to reduce the grain size of rhenium-tungsten alloys. This, in turn, improves the tensile strength of the tungsten wire.
[0078] Furthermore, as mentioned above, when the rhenium content becomes too high, thinning of the tungsten wire while maintaining high tensile strength will result in wire breakage and difficulty in drawing long strands. Conventionally, to improve the tensile strength of tungsten wire, it is necessary to include 10% or more rhenium. With such a high rhenium content, it is difficult to achieve tungsten wire diameters below 100 μm. Moreover, according to this embodiment, it has been found that even with a rhenium content of at most 0.5% or 1% by weight, and even with tungsten wire containing 99.5% or more by weight, higher tensile strength than previously achieved can be obtained.
[0079] [Manufacturing method of tungsten wire]
[0080] Next, regarding the manufacturing method of the tungsten wire 10 in this embodiment, using... Figure 5 Please provide an explanation. Figure 5 This is a flowchart illustrating the manufacturing method of the tungsten wire 10 according to this embodiment.
[0081] like Figure 5 As shown, first, a tungsten ingot is prepared (S10). Specifically, a tungsten ingot is made by pressing and sintering an aggregate of tungsten powder.
[0082] Furthermore, in the case of manufacturing tungsten wire 10 formed of tungsten alloy, a mixture obtained by mixing tungsten powder with metal powder (e.g., rhenium powder) in a predetermined ratio is prepared to replace the aggregate of tungsten powder. The average particle size of the tungsten powder and rhenium powder is, for example, in the range of 3 μm or more and 4 μm or less, but is not limited thereto.
[0083] Next, the tungsten ingot is subjected to die forging (S12). Specifically, the tungsten ingot is stretched by forging and compressing it from all sides, forming it into a linear tungsten wire. Instead of die forging, rolling can also be used.
[0084] For example, tungsten ingots with a diameter of approximately 15 mm to 25 mm are formed into tungsten wires with a diameter of approximately 3 mm through repeated forging processes. During the forging process, annealing is performed to ensure machinability in subsequent processing. For example, annealing at 2400°C is performed for diameters of 8 mm to 10 mm. However, to ensure the tensile strength resulting from grain refinement, annealing is not performed in forging processes with diameters less than 8 mm.
[0085] Next, the tungsten wire is heated at 900°C before heating and drawing (S14). Specifically, the tungsten wire is heated directly using a burner or the like. By heating the tungsten wire, an oxide layer is formed on its surface, preventing wire breakage during subsequent heating and drawing.
[0086] Next, heated wire drawing (S16) is performed. Specifically, one or more drawing dies are used to draw tungsten wire while heating, i.e., tungsten wire drawing (fine wire drawing). The heating temperature is, for example, 1000°C. Furthermore, the higher the heating temperature, the better the machinability of the tungsten wire, thus making wire drawing easier. Heated wire drawing is repeated while changing the drawing die. The reduction rate of cross-sectional area of the tungsten wire obtained by drawing in one pass using a single drawing die is, for example, 10% or more and 40% or less. A lubricant obtained by dispersing graphite in water can also be used in the heated wire drawing process.
[0087] Repeatedly perform heating and drawing (S16) until a tungsten wire of the desired diameter is obtained (No in S18). The desired wire diameter here is the wire diameter at the stage before the final drawing process (S20), for example, about 712 μm or less.
[0088] During repeated heating and drawing processes, a drawing die with a smaller aperture than that used in previous drawing processes can be used. Furthermore, during these repeated heating and drawing processes, the tungsten wire is heated to a lower temperature than the heating temperature used in previous drawing processes. For example, the heating temperature in the drawing process preceding the final drawing process is lower than the previous heating temperature, for example, 400°C, which helps to refine the grain size.
[0089] If the desired tungsten wire diameter is obtained and the next drawing process is the final step ("Yes" in S18), room temperature drawing is performed with a processing rate of 70% or higher (S20). That is, by drawing the tungsten wire without heating, further grain refinement is achieved. Furthermore, room temperature drawing ensures that the crystal orientation is aligned along the processing axis (specifically, the direction parallel to the wire axis P). Room temperature is, for example, a temperature ranging from 0°C to 50°C, with 30°C as an example. Specifically, multiple drawing dies with different apertures are used to draw the tungsten wire. A water-soluble liquid lubricant is used in room temperature drawing. Since no heating is performed in room temperature drawing, liquid evaporation is suppressed. Therefore, the liquid lubricant can function effectively. Compared to the traditional tungsten wire processing method of heating and drawing at temperatures above 600°C, this method does not heat the tungsten wire. In addition, it cools the wire with a liquid lubricant while processing, thereby suppressing dynamic recovery and dynamic recrystallization, preventing wire breakage, promoting grain refinement, and achieving high tensile strength.
[0090] The processing rate is expressed by the wire diameter Db before room temperature drawing and the wire diameter Da immediately after room temperature drawing, using the following formula (4).
[0091] (4) Processing rate = {1 - (Da / Db)} 2}×100
[0092] As can be seen from equation (4), the larger the wire diameter decreases through room temperature drawing, the larger the processing rate becomes. For example, even if the wire diameter Db is the same after room temperature drawing, the larger the processing rate, the smaller the wire diameter Da becomes after room temperature drawing. By increasing the processing rate, the degree of fineness of the tungsten wire resulting from room temperature drawing increases, that is, finer tungsten wire can be obtained. The processing rate of room temperature drawing is 70% or more, but it can also be 80% or more, 90% or more, or even 95% or more.
[0093] To obtain tungsten wire with a diameter greater than 100 μm after room temperature drawing, simply increase the wire diameter before room temperature drawing. For example, to obtain tungsten wire with a processing rate of 70% and a wire diameter of approximately 100 μm after room temperature drawing, according to formula (4), simply start room temperature drawing of tungsten wire with a wire diameter of approximately 183 μm.
[0094] The processing rate of room temperature wire drawing can be changed by adjusting the shape and number of dies used in the wire drawing process. In addition, as for the wire drawing dies used, for example, superhard dies are used when the wire diameter is below 0.38mm, sintered diamond dies are used in the range of 0.38mm to 0.18mm, and single crystal diamond dies are used in the range of 0.18mm to 0.018mm.
[0095] Finally, for tungsten wires of the desired diameter formed by room-temperature drawing, electrolytic polishing (S22) is performed to fine-tune the diameter. Electrolytic polishing is performed, for example, by generating a potential difference between the tungsten wire and the counter electrode while the tungsten wire and the counter electrode are immersed in an electrolyte such as an aqueous sodium hydroxide solution.
[0096] Through the above processes, the tungsten wire 10 of this embodiment can be manufactured. The length of the tungsten wire 10 immediately after manufacturing through the above processes is, for example, 50 km or more, and it can be used industrially. The tungsten wire 10 can also be cut to suitable lengths depending on the method used, and can also be used in the shape of a needle or rod. Thus, in this embodiment, the tungsten wire 10 can be mass-produced industrially and can be used in various fields such as medical needles, saw wires, and screen printing grids.
[0097] The tungsten wire 10 of Examples 1 to 11 described above is a tungsten wire manufactured through the above processes. The tungsten wires of each example can be manufactured by appropriately adjusting the rhenium content, the processing rate of room temperature drawing, and the wire diameter.
[0098] Furthermore, the various processes shown in the method for manufacturing tungsten wire 10 can be performed in series, for example. Specifically, the multiple drawing dies used in step S16 are arranged on the production line in order of decreasing aperture. Additionally, a heating device such as a burner is arranged between each drawing die. Furthermore, an electrolytic polishing device can also be arranged between each drawing die. Downstream of the drawing die used in step S16 (towards the next process), the multiple drawing dies used in step S20 are arranged in order of decreasing aperture, and an electrolytic polishing device is arranged downstream of the drawing die with the smallest aperture. Alternatively, each process can also be performed individually.
[0099] [Sawing wire]
[0100] The tungsten wire 10 in this embodiment is, for example, as shown in the example... Figure 6 As shown, the saw wire 2 can be used as a cutting device 1 for cutting objects such as silicon ingots or concrete. Figure 6 This is a perspective view showing the cutting device 1 of this embodiment.
[0101] like Figure 6 As shown, the cutting device 1 is a multi-wire saw with sawing wires 2. The cutting device 1 manufactures wafers, for example, by cutting the ingot 30 into thin plates. The ingot 30 is, for example, a silicon ingot made of monocrystalline silicon. Specifically, the cutting device 1 cuts the ingot 30 with multiple sawing wires 2, thereby manufacturing multiple silicon wafers simultaneously.
[0102] Furthermore, ingot 30 is not limited to silicon ingots; it can also be other ingots such as silicon carbide or sapphire. Alternatively, the object to be cut using the cutting device 1 can also be concrete or glass.
[0103] In this embodiment, the saw wire 2 includes a tungsten wire 10. Specifically, the saw wire 2 is the tungsten wire 10 itself in this embodiment. Alternatively, the saw wire 2 may also include a tungsten wire 10 and a plurality of abrasive grains attached to the surface of the tungsten wire 10.
[0104] like Figure 6 As shown, the cutting device 1 further includes two guide rollers 3, a support 4, and a tension easing device 5.
[0105] On the two guide rollers 3, one saw wire 2 is wound multiple times. Here, for ease of explanation, one turn of the saw wire 2 is considered as one saw wire 2, and the explanation is given in the manner that multiple saw wires 2 are wound on the two guide rollers 3. That is, in the following explanation, multiple saw wires 2 form one continuous saw wire 2. Alternatively, the multiple saw wires 2 can also be multiple separate saw wires.
[0106] Two guide rollers 3 rotate independently while the multiple saw wires 2 are stretched straight under a specified tension, thereby causing the multiple saw wires 2 to rotate at a specified speed. The multiple saw wires 2 are parallel to each other and arranged at equal intervals. Specifically, each of the two guide rollers 3 has multiple slots for inserting the saw wires 2 at a specified interval. The spacing of the slots is determined according to the thickness of the wafer to be cut. The width of the slots is approximately the same as the wire diameter of the saw wire 2.
[0107] Alternatively, the cutting device 1 may have three or more guide rollers 3. Multiple saw lines 2 may also be wound around the three or more guide rollers 3.
[0108] The support part 4 supports the spindle 30, which is the object to be cut. The support part 4 presses the spindle 30 toward the multiple saw lines 2, thereby cutting the spindle 30 by the multiple saw lines 2.
[0109] The tension easing device 5 is a device that eases the tension applied to the saw wire 2. For example, the tension easing device 5 is an elastic body such as a coil spring or a leaf spring. Figure 6As shown, for example, one end of the tension easing device 5, which is a helical spring, is connected to the guide roller 3, and the other end is fixed to a predetermined wall surface. The tension easing device 5 can ease the tension applied to the saw wire 2 by adjusting the position of the guide roller 3.
[0110] Additionally, although not shown, the cutting device 1 can also be a free abrasive cutting device, equipped with a supply device for supplying slurry to the saw wire 2. The slurry is a substance in which abrasive particles are dispersed in a cutting fluid such as a cooling medium. By allowing the abrasive particles contained in the slurry to adhere to the saw wire 2, the spindle 30 can be easily cut.
[0111] The saw wire 2, which has high tensile strength tungsten wire 10, can be stretched on the guide roller 3 with strong tension. As a result, the vibration of the saw wire 2 during the cutting of the spindle 30 can be suppressed, thus reducing the wear of the spindle 30.
[0112] [Silk screen]
[0113] Furthermore, the tungsten wire 10 of this embodiment can be used as a tungsten wire for screen printing. Specifically, as... Figure 7 As shown, it can also be used as the wire of a metal mesh such as screen 40 used in screen printing.
[0114] Figure 7 This is a diagram representing a 40mm screen. Figure 7 In this illustration, only a portion of the mesh of the screen 40 is shown schematically, but the entire screen 40 is mesh-like. For example, the screen 40 has multiple tungsten threads 10 woven as warp and weft yarns.
[0115] The screen 40 has multiple openings 42. The openings 42 are the portions through which ink passes during screen printing. By blocking a portion of the openings 42 with an emulsion or resin (e.g., polyimide), non-passing portions are formed where ink cannot pass. By patterning the shape of the non-passing portions in any shape, screen printing can be performed in the desired shape.
[0116] Alternatively, the tungsten wire for screen printing may also have a tungsten wire 10 and a covering layer covering the surface of the tungsten wire 10. The covering layer is provided, for example, to improve the holding power of emulsions, etc.
[0117] [Effects, etc.]
[0118] As described above, the tungsten wire 10 of this embodiment is formed of tungsten or a tungsten alloy. The average width of the surface grains of the tungsten wire 10 in the direction perpendicular to the wire axis P is 98 nm or less. The tensile strength of the tungsten wire 10 is 3900 MPa or more. The wire diameter of the tungsten wire 10 is greater than 100 μm and less than 225 μm.
[0119] Therefore, even in tungsten wires with a diameter greater than 100μm, it is possible to achieve a higher tensile strength than that of typical piano wire.
[0120] Furthermore, for example, in the tungsten wire 10 of this embodiment, the wire diameter is 18 μm or more and 225 μm or less. When the tensile strength is set to T [MPa] and the wire diameter is set to D [mm], T ≥ 4758 × D 2 -7258.3×D+5275.5 holds true.
[0121] In the past, tensile strength could be increased by reducing the wire diameter, but according to this embodiment, tensile strength higher than that of the past can be achieved with each wire diameter.
[0122] Furthermore, for example, the tungsten content in tungsten wire 10 is more than 99% by weight.
[0123] Therefore, even in the case of alloying, the content of alloy materials such as rhenium can be set to less than 1%. For example, by reducing the rhenium content, it is easy to make the wire thinner while maintaining its strength, thus enabling the production of tungsten wires that are thinner and have higher tensile strength than before.
[0124] In addition, the tungsten wire 10 can be used not only in saw wire 2 or wire mesh 40, but also in medical needles or examination probes. Furthermore, the tungsten wire 10 can also be used as reinforcing wire for elastic components such as tires, conveyor belts, or conduits. For example, a tire has multiple tungsten wires 10 bundled into layers as a belt or tire carcass cord.
[0125] (other)
[0126] The tungsten wire, saw wire, and tungsten wire for screen printing of the present invention have been described above based on the above embodiments, but the present invention is not limited to the above embodiments.
[0127] For example, the metal contained in a tungsten alloy may not be rhenium. That is, a tungsten alloy may be an alloy of tungsten and one or more metals different from tungsten. Metals different from tungsten may be transition metals such as iridium (Ir), ruthenium (Ru), or osmium (Os). The content of these metals may be, for example, 0.1% by weight or more and 1% by weight, but is not limited thereto. For example, the content of metals different from tungsten may be less than 0.1% by weight or greater than 1% by weight. The same applies to rhenium.
[0128] Furthermore, for example, tungsten wire 10 can also be formed from tungsten doped with potassium (K). The doped potassium is present in the grain boundaries of the tungsten. The potassium (K) dispersed in the grain boundaries suppresses crystal coarsening during high-temperature heating and wire drawing, but does not cause crystal coarsening during processing in room-temperature wire drawing. Therefore, the amount of potassium (K) can be, for example, any value in the range of 0.005% by weight or more and 0.01% by weight or less. In the case of potassium-doped tungsten wire, it is also possible to achieve tungsten wire with a tensile strength higher than that of piano wire, similar to the case of tungsten alloy wire.
[0129] Potassium-doped tungsten wires can be manufactured by using potassium-doped tungsten powder instead of tungsten powder, using the same manufacturing method as in the embodiments.
[0130] In addition, for example, an oxide film or a nitride film may be applied to the surface of the tungsten wire 10.
[0131] Furthermore, this invention also includes various modifications to the embodiments that would be conceived by those skilled in the art, or embodiments achieved by arbitrarily combining the constituent elements and functions of each embodiment without departing from the spirit of the invention.
[0132] Explanation of symbols
[0133] 2. Saw wire
[0134] 10 Tungsten wire
[0135] 40 mesh
Claims
1. A tungsten wire which is a tungsten wire formed of tungsten or a tungsten alloy, an average value of widths of surface grains in a direction perpendicular to a spool of the tungsten wire is 79 nm or less, a tensile strength of the tungsten wire is 4500 MPa or more, a wire diameter of the tungsten wire is 104 μm or less, in a case where the tensile strength is set to T and the wire diameter is set to D, T ≥ 4758 x D 2 - 7258.3 x D + 5275.5 holds, a unit of the tensile strength is MPa and a unit of the wire diameter is mm.
2. The tungsten wire of claim 1, wherein, the wire diameter of the tungsten wire is 18 μm or more.
3. The tungsten wire of claim 1 or 2, wherein, a content rate of tungsten in the tungsten wire is 99% by weight or more.
4. A sawing wire provided with the tungsten wire according to any one of claims 1 to 3.
5. A tungsten wire for screen printing provided with the tungsten wire according to any one of claims 1 to 3.
Citation Information
Patent Citations
Medical needle
JP2014169499A
A tungsten wire, a screen and a tungsten fiber
CN107538948A
Saw wire and cutting apparatus
CN108858838A