Graphene / aluminum composite conductor and preparation method thereof

By employing graphite orientation treatment and axial drawing processes, the problem of poor bonding effect of graphene in aluminum-based composite materials was solved, resulting in graphene/aluminum composite materials with high conductivity and high strength. This simplified the preparation process and reduced costs.

CN118147492BActive Publication Date: 2026-11-20NINGBO GRAPHENE INNOVATION CENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410306064.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-18
Publication Date
2026-11-20
Estimated Expiration
2044-03-18

AI Technical Summary

Technical Problem

In the existing technology, the process of adding graphene to aluminum-based composite materials has problems such as low maturity, complex process and high cost, resulting in limited improvement in the conductivity of aluminum alloys, and the bonding effect between graphene and aluminum alloys is not good, making it difficult to achieve both high conductivity and high strength.

Method used

By employing graphite orientation treatment and axial drawing processes, oriented graphite/aluminum mixed powder is filled into an aluminum tube protective sleeve. Through multiple drawing and annealing processes, graphene is ensured to peel off layer by layer from the graphite surface. Combined with aluminum powder particles, the adhesion between graphene and aluminum is enhanced, avoiding agglomeration and forming a highly dense and highly conductive graphene/aluminum composite material.

Benefits of technology

The preparation process of graphene has been simplified, the cost has been reduced, the exfoliation efficiency and adhesion of graphene in aluminum-based composite materials have been improved, agglomeration has been avoided, and graphene/aluminum composite materials with high conductivity and high strength have been achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118147492B_ABST
    Figure CN118147492B_ABST
Patent Text Reader

Abstract

This invention discloses a graphene / aluminum composite conductor and its preparation method. A graphite dispersion and an aluminum powder dispersion are mixed, and the graphite is oriented using liquid nitrogen freezing technology. After drying, an oriented graphene / aluminum mixed powder is obtained. The powder is then protected by an inclined aluminum tube, which contains the oriented graphene / aluminum mixed powder. The mixture is then axially drawn and annealed. The combination of graphite orientation treatment and the inclined aluminum tube protection method results in a 0°~20° angle between the graphite sheets and the drawing direction. This allows the graphene to be peeled off from the graphite surface with relatively low shear stress, reducing the difficulty of graphene peeling and simplifying the graphene preparation process. The presence of aluminum powder particles provides greater adhesion to the graphite, facilitating the peeling of graphene from the graphite surface. The physical combination of graphene and aluminum allows the aluminum matrix to provide a large number of electrons, while graphene, with its ultra-high carrier transport rate, becomes the runway for electron movement. The synergistic effect of graphene and aluminum improves the electrical conductivity of the material. The aluminum-based composite material containing directionally aligned graphite achieves a conductivity of 67% IACS, an improvement of over 10% compared to pure aluminum. This invention solves the bottleneck problem limiting the low-cost, large-scale preparation of highly conductive graphene / aluminum composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials science and relates to a graphene / aluminum composite conductor and its preparation method. Background Technology

[0002] With the rise in international copper prices, the price of traditional copper-based conductors is also gradually increasing. Exploring materials with low cost and high conductivity has become urgent. Aluminum has electrical conductivity second only to gold, silver, and copper, and also boasts advantages such as low density and high strength. Therefore, aluminum is trending towards replacing copper in electrical appliance manufacturing, wire and cable, and the radio industry.

[0003] Currently, common processes for improving the conductivity of aluminum alloys include adding rare earth elements, boronizing treatment, and optimizing processing techniques. Adding appropriate amounts of rare earth elements to aluminum alloys can significantly increase conductivity while maintaining strength; however, rare earth elements are expensive, significantly increasing raw material costs. Adding boron (B) for boronizing treatment causes elements such as Ti and V in the aluminum alloy melt to react with B, producing TiB2 and VB2 precipitates at the bottom of the melt, reducing the content of impurity elements and improving the conductivity of the aluminum alloy, but at the cost of reduced material strength. Commonly used processing optimization methods include artificial aging and heat treatment, which aim to improve the internal structure of the alloy and reduce the damage to conductivity caused by lattice distortion due to solid solution of alloying elements in the aluminum lattice, thus achieving higher conductivity. However, processing optimization cannot completely eliminate the negative impact of solid solution elements on conductivity, and the conductivity of the alloy cannot exceed that of pure aluminum.

[0004] Graphene, as a two-dimensional material, has a strength of up to 1.01 TPa, and the charge mobility of monolayer graphene at room temperature is as high as 15,000 cm⁻¹. 2 / (V·s), graphene, with its excellent properties, is used to improve strength and conductivity. Current research on graphene-reinforced aluminum-based composites shows that uniformly adding graphene to a certain mass enhances the conductivity of the composite. However, domestic and international processes for improving the conductivity of aluminum-based composites with graphene addition still face challenges such as low maturity, complex processes, and high costs, limiting the development of material systems. Patent document 1 (CN 106128545 A) discloses a graphene-core electrical conductor and its preparation method. This involves filling graphene particles into a sleeve made of sheathing material and drawing it to form a graphene core and sheath composite. An annealing treatment and repeated drawing are then used to obtain a graphene-core electrical conductor. The problem with this process is that graphene in contact with the metal inner wall of the sleeve can be peeled off under the adhesion force of the metal wall and the pulling shear force; however, most of the graphite has no physical contact with the metal, and the solid lubrication between graphites causes slippage under external force, preventing most of the shear force from peeling off the graphite. Therefore, graphite has a weak exfoliation effect, which is not conducive to graphite exfoliation and composite with the tube wall metal. Patent document 2 (CN 115449672 A) discloses a high-strength, high-conductivity graphene-reinforced aluminum-based conductive wire and its preparation method. First, graphene and aluminum powder are ball-milled and mixed, then subjected to rotary friction extrusion, and finally drawn into a high-strength, high-conductivity graphene-reinforced aluminum-based wire. The ball-milling method easily causes the sheet-like graphene to agglomerate, resulting in wrinkles. During processing, the agglomerated graphene leaves voids in the aluminum matrix, hindering electron transport within the matrix and impairing conductivity. Furthermore, all methods for preparing graphene, including oxidation-reduction, mechanical exfoliation, and microwave methods, have certain processing costs, leading to increased costs and hindering product commercialization. Summary of the Invention

[0005] To address the aforementioned problems, this invention discloses a graphene / aluminum composite conductor and its preparation method.

[0006] This invention is achieved through the following technical solution: A graphene / aluminum-based composite conductor is composed of the following alloy components by mass percentage: graphene 1%-10%, Si ≤0.03%, Fe ≤0.03%, each of the remaining impurity elements ≤0.01%, and the balance being Al.

[0007] The preparation method of the graphene / aluminum-based composite material described above includes the following steps: First, fill the aluminum tube protective sleeve with oriented graphene / aluminum mixed powder; second, axially pull the protective sleeve containing the mixed powder, and then anneal it in a vacuum or inert gas environment; then change the mold and pull it again, and anneal it again, repeating the process.

[0008] Preferably, the method for preparing the above-mentioned oriented graphite / aluminum mixed powder includes the following steps: (1) Preparation of aluminum powder dispersion: Disperse spherical aluminum powder with a particle size distribution of 80-300 mesh in 75% alcohol by volume, and perform ultrasonic treatment to obtain aluminum powder dispersion; (2) Preparation of graphite dispersion: Disperse thin-layer graphite powder with a two-dimensional size of 10-100 micrometers in 75% alcohol by volume, and sonicate it to form a uniform solution to obtain graphene dispersion. (3) Mixing aluminum powder dispersion and graphite dispersion: Mix aluminum powder dispersion and graphite dispersion, and sonicate in a water bath for 5 to 10 minutes at a frequency of 10KHz~100KHz, and then sonicate at a power of 200W for 30 minutes to obtain graphite / aluminum powder mixed dispersion. (4) Oriented treatment and drying of graphite: The mixed dispersion obtained in step (3) is rapidly frozen to form a mixture of aluminum, graphene and solid alcohol. The mixture is placed in a freeze dryer and dried at -100℃ for 24h~36h to obtain oriented graphite / aluminum mixed powder.

[0009] Preferably, the aluminum tube protective sleeve is filled with oriented graphite / aluminum mixed powder by inserting the aluminum tube protective sleeve into the dried mixed powder at an angle of 70° to 90° relative to the vertical direction, and after filling with powder, sealing both ends of the aluminum tube protective sleeve.

[0010] Preferably, the annealing environment is a vacuum or inert gas environment, and the annealing temperature is 100℃~300℃.

[0011] Preferably, during the drawing process, the drawing direction is along the axial direction of the aluminum tube protective sleeve, and the deformation amount of a single drawing is between 10% and 15%, ultimately obtaining a metal wire with a diameter ≤10mm.

[0012] Preferably, the ultrasonic treatment of the aluminum powder dispersion and the graphite dispersion is carried out at an ultrasonic frequency of 10KHz~100KHz and an ultrasonic time of 30min~60min.

[0013] Beneficial effects (1) The present invention uses the orientation treatment and drawing process of graphite to prepare materials, combining aluminum powder particles with oriented graphite, making it easier for graphene to peel off layer by layer from the graphite surface during the drawing process, simplifying the graphene preparation process, reducing the graphene preparation cost, and having a simple process, dense material and high electrical conductivity, avoiding the disadvantages of high cost of rare earth addition to aluminum alloy and the inability of boronizing treatment to break through the conventional electrical conductivity of pure aluminum.

[0014] (2) When the angle between the graphite orientation and the drawing direction is 0°, the shear stress required to peel graphene off the graphite surface is minimized. Since the orientation-treated graphite does not agglomerate and spreads horizontally, the orientation-oriented graphite will coat the surface of the aluminum powder particles horizontally during the drying process. Meanwhile, considering the difficulty in controlling the horizontal direction of the aluminum tube protective sleeve in actual production, angular deviations are permissible. The aluminum tube protective sleeve is inserted at a 70°~90° angle relative to the vertical direction and filled with mixed powder, maintaining an angle of 0°~20° between the orientation-oriented graphite and the axial direction of the aluminum tube protective sleeve. During the drawing process, the orientation-oriented graphite forms an angle of 0°~20° with the drawing direction, allowing graphene to peel off from the graphite surface under relatively small shear stress, thus improving the graphene peeling efficiency.

[0015] (3) The presence of aluminum powder particles on the graphite surface increases the interaction force between the graphite and the tube wall, providing greater adhesion for the exfoliation of graphite sheets and facilitating the exfoliation of graphene on the graphite surface. After graphene is exfoliated on the surface of aluminum powder particles, it will not agglomerate due to the squeezing force of the surrounding metal particles and aluminum protective sleeve, thus avoiding the void phenomenon in the aluminum matrix caused by graphene agglomeration, thereby improving the density and conductivity of graphene-reinforced aluminum matrix composites. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of the process flow; Figure 2 Schematic diagram of directional graphite processing; Figure 3 A schematic diagram illustrating the principle of graphene shedding from the inner wall of an aluminum tube during the drawing process; Figure 4 This is a schematic diagram illustrating the relative motion of mixed powders during the drawing process to peel off graphene. Figure 5 This is a schematic diagram of the technical route. Detailed Implementation

[0017] The embodiments of the present invention are described in detail below. These embodiments are implemented based on the technical solution of the present invention, and provide detailed implementation methods and specific operation processes. However, the scope of protection of the present invention is not limited to the following embodiments.

[0018] Comparative Example 1 A graphene / aluminum composite conductor is composed of the following alloy components by mass percentage: graphene 5.00%, Si 0.03%, Fe 0.03%, each of the remaining impurity elements ≤0.01%, and the balance being Al.

[0019] First, the preparation method of graphite / aluminum mixed powder includes the following steps: (1) Preparation of aluminum powder dispersion: Disperse spherical aluminum powder with a particle size distribution of 125 mesh in 75% alcohol by volume, and perform ultrasonic treatment at a frequency of 50KHz for 45min to obtain aluminum powder dispersion. (2) Preparation of graphite dispersion: 50-micron thin-layer graphite powder with a two-dimensional size is dispersed in 75% alcohol by volume and subjected to ultrasonic treatment at a frequency of 50 kHz for 45 min to form a uniform solution and obtain graphene dispersion. (3) Mixing aluminum powder dispersion and graphite dispersion: Mix aluminum powder dispersion and graphite dispersion, sonicate in water bath for 7 min at a frequency of 50 kHz, and then sonicate at a power of 200 W for 30 min to obtain graphite / aluminum powder mixed dispersion. (4) Drying of graphite / aluminum powder mixed dispersion: The mixed dispersion obtained in step (3) is dried in an oven at room temperature for 36 hours to obtain mixed aluminum powder particles.

[0020] The graphite / aluminum mixed powder is loaded into the aluminum tube protective sleeve in any direction. After the tube is filled with powder particles, both ends of the aluminum tube protective sleeve are sealed.

[0021] Secondly, the protective sleeve containing the mixed powder is axially drawn, and then annealed in a vacuum or inert gas environment. Then, the die is changed, and the process is repeated with drawing and annealing again in a vacuum or inert gas environment at a temperature of 100℃. During the drawing process, the drawing direction is along the axial direction of the aluminum tube protective sleeve, and the deformation in a single drawing is between 10% and 15%. This process is repeated until a metal wire with a diameter ≤10mm is obtained.

[0022] Example 1 A graphene / aluminum composite conductor is composed of the following alloy components by mass percentage: graphene 1.00%, Si 0.03%, Fe 0.03%, each of the remaining impurity elements ≤0.01%, and the balance being Al.

[0023] The preparation method of the above-mentioned conductor material includes the following steps: First, fill the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder; second, axially draw the protective sleeve containing the mixed powder, and then anneal it in a vacuum or inert gas environment; then change the mold and draw it again, and anneal it again, and repeat the process.

[0024] The method for preparing the above-mentioned oriented graphite / aluminum mixed powder includes the following steps: (1) Preparation of aluminum powder dispersion: Disperse spherical aluminum powder with a particle size distribution of 300 mesh in 75% alcohol by volume, and perform ultrasonic treatment at a frequency of 10KHz for 30min to obtain aluminum powder dispersion. (2) Preparation of graphite dispersion: Graphite powder with a two-dimensional size of 100 micrometers is dispersed in alcohol with a volume fraction of 75% and subjected to ultrasonic treatment at a frequency of 10 kHz for 30 min to form a uniform solution and obtain graphene dispersion. (3) Mixing aluminum powder dispersion and graphite dispersion: Mix aluminum powder dispersion and graphite dispersion, sonicate in water bath for 5 min at a frequency of 10KHz, and then sonicate at a power of 200W for 30 min to obtain graphite / aluminum powder mixed dispersion. (4) Oriented treatment and drying of graphite: The mixed dispersion obtained in step (3) is quick-frozen to form a mixture of aluminum, graphene and solid alcohol. The mixture is placed in a freeze dryer and dried at -100℃ for 36 hours to obtain oriented graphite / aluminum mixed powder.

[0025] The above method of filling the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder is as follows: the aluminum tube protective sleeve is inserted into the dried mixed powder at a 70°~90° angle relative to the vertical direction, and after filling with powder, the two ends of the aluminum tube protective sleeve are sealed.

[0026] The annealing process described above is performed in a vacuum or inert gas environment at a temperature of 100°C.

[0027] In the above drawing process, the drawing direction is along the axial direction of the aluminum tube protective sleeve, and the deformation of a single drawing is between 10% and 15%, finally obtaining a metal wire with a diameter ≤10mm.

[0028] Example 2 A graphene / aluminum composite conductor is composed of the following alloy components by mass percentage: graphene 3.00%, Si 0.03%, Fe 0.03%, each of the remaining impurity elements ≤0.01%, and the balance being Al.

[0029] The preparation method of the aluminum-based composite material described above includes the following steps: First, fill the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder; second, axially pull the protective sleeve containing the mixed powder, and then anneal it in a vacuum or inert gas environment; then change the mold and pull it again, and anneal it again, and repeat the process.

[0030] The method for preparing the above-mentioned oriented graphite / aluminum mixed powder includes the following steps: (1) Preparation of aluminum powder dispersion: Spherical aluminum powder with a particle size distribution of 175 mesh is dispersed in 75% alcohol by volume and subjected to ultrasonic treatment at a frequency of 30KHz for 40min to obtain aluminum powder dispersion. (2) Preparation of graphite dispersion: 80-micron thin-layer graphite powder with a two-dimensional size is dispersed in 75% alcohol by volume and subjected to ultrasonic treatment at a frequency of 30 kHz for 40 min to form a uniform solution and obtain graphene dispersion. (3) Mixing aluminum powder dispersion and graphite dispersion: Mix aluminum powder dispersion and graphite dispersion, sonicate in water bath for 6 minutes at a frequency of 30KHz, and then sonicate at a power of 200W for 30 minutes to obtain graphite / aluminum powder mixed dispersion. (4) Oriented treatment and drying of graphite: The mixed dispersion obtained in step (3) is quick-frozen to form a mixture of aluminum, graphene and solid alcohol. The mixture is placed in a freeze dryer and dried at -100℃ for 36 hours to obtain oriented graphite / aluminum mixed powder.

[0031] The above method of filling the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder is as follows: the aluminum tube protective sleeve is inserted into the dried mixed powder at a 70°~90° angle relative to the vertical direction, and after filling with powder, the two ends of the aluminum tube protective sleeve are sealed.

[0032] The annealing process described above is performed in a vacuum or inert gas environment at a temperature of 100°C.

[0033] In the above drawing process, the drawing direction is along the axial direction of the aluminum tube protective sleeve, and the deformation of a single drawing is between 10% and 15%, ultimately resulting in a metal wire with a diameter of ≤10mm.

[0034] Example 3 A graphene / aluminum composite conductor is composed of the following alloy components by mass percentage: graphene 5.00%, Si 0.03%, Fe 0.03%, each of the remaining impurity elements ≤0.01%, and the balance being Al.

[0035] The method for preparing the conductor material described above includes the following steps: First, a graphite / aluminum mixed powder is filled into an aluminum tube protective sleeve in an oriented manner; second, the protective sleeve containing the mixed powder is axially drawn, and then annealed in a vacuum or inert gas environment; then the mold is changed and the drawing and annealing are repeated.

[0036] The method for preparing the above-mentioned oriented graphite / aluminum mixed powder includes the following steps: (1) Preparation of aluminum powder dispersion: Disperse spherical aluminum powder with a particle size distribution of 125 mesh in 75% alcohol by volume, and perform ultrasonic treatment at a frequency of 50KHz for 45min to obtain aluminum powder dispersion. (2) Preparation of graphite dispersion: 60-micron thin-layer graphite powder with a two-dimensional size is dispersed in 75% alcohol by volume and subjected to ultrasonic treatment at a frequency of 50 kHz for 45 min to form a uniform solution and obtain graphene dispersion. (3) Mixing aluminum powder dispersion and graphite dispersion: Mix aluminum powder dispersion and graphite dispersion, sonicate in water bath for 7 min at a frequency of 50 kHz, and then sonicate at a power of 200 W for 30 min to obtain graphite / aluminum powder mixed dispersion. (4) Graphite orientation treatment and drying: The mixed dispersion obtained in step (3) is quick-frozen to form a mixture of aluminum, graphene and solid alcohol. The mixture is placed in a freeze dryer and dried at -100℃ for 36 hours to obtain mixed aluminum powder particles.

[0037] The above method of filling the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder is as follows: the aluminum tube protective sleeve is inserted into the dried mixed powder at a 70°~90° angle relative to the vertical direction, and after filling with powder, the two ends of the aluminum tube protective sleeve are sealed.

[0038] The annealing process described above is performed in a vacuum or inert gas environment at a temperature of 200°C.

[0039] In the above drawing process, the drawing direction is along the axial direction of the aluminum tube protective sleeve, and the deformation of a single drawing is between 10% and 15%, finally obtaining a metal wire with a diameter ≤10mm.

[0040] Example 4 A graphene / aluminum composite conductor is composed of the following alloy components by mass percentage: graphene 6.00%, Si 0.03%, Fe 0.03%, each of the remaining impurity elements ≤0.01%, and the balance being Al.

[0041] The method for preparing the conductor material described above includes the following steps: First, a graphite / aluminum mixed powder is filled into an aluminum tube protective sleeve in an oriented manner; second, the protective sleeve containing the mixed powder is axially drawn, and then annealed in a vacuum or inert gas environment; then the mold is changed and the drawing and annealing are repeated.

[0042] The above-mentioned method for preparing oriented graphite / aluminum mixed powder includes the following steps: (1) Preparation of aluminum powder dispersion: Disperse spherical aluminum powder with a particle size distribution of 125 mesh in 75% alcohol by volume, and perform ultrasonic treatment at a frequency of 70KHz for 50min to obtain aluminum powder dispersion. (2) Preparation of graphite dispersion: Graphite powder with a two-dimensional size of 40 micrometers is dispersed in alcohol with a volume fraction of 75% and subjected to ultrasonic treatment at a frequency of 70KHz for 50min to form a uniform solution and obtain graphene dispersion. (3) Mixing aluminum powder dispersion and graphite dispersion: Mix aluminum powder dispersion and graphite dispersion, sonicate in water bath for 8 minutes at a frequency of 70KHz, and then sonicate at a power of 200W for 30 minutes to obtain graphite / aluminum powder mixed dispersion. (4) Oriented treatment and drying of graphite: The mixed dispersion obtained in step (3) is quick-frozen to form a mixture of aluminum, graphene and solid alcohol. The mixture is placed in a freeze dryer and dried at -100℃ for 36 hours to obtain oriented graphite / aluminum mixed powder.

[0043] The above method of filling the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder is as follows: the aluminum tube protective sleeve is inserted into the dried mixed powder at a 70°~90° angle relative to the vertical direction, and after filling with powder, the two ends of the aluminum tube protective sleeve are sealed.

[0044] The annealing process described above is performed in a vacuum or inert gas environment at a temperature of 200°C.

[0045] In the above drawing process, the drawing direction is along the axial direction of the aluminum tube protective sleeve, and the deformation of a single drawing is between 10% and 15%, finally obtaining a metal wire with a diameter ≤10mm.

[0046] Example 5 A graphene / aluminum composite conductor method comprises the following alloy components by mass percentage: 8.00% graphene, 0.03% Si, 0.03% Fe, with each of the remaining impurity elements ≤0.01%, and the balance being Al.

[0047] The preparation method of the above-mentioned conductor material includes the following steps: First, fill the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder; second, axially draw the protective sleeve containing the mixed powder, and then anneal it in a vacuum or inert gas environment; then change the mold and draw it again, and anneal it again, and repeat the process.

[0048] The method for preparing the above-mentioned oriented graphite / aluminum mixed powder includes the following steps: (1) Preparation of aluminum powder dispersion: Disperse spherical aluminum powder with a particle size distribution of 100 mesh in 75% alcohol by volume, and perform ultrasonic treatment at a frequency of 90KHz for 55min to obtain aluminum powder dispersion. (2) Preparation of graphite dispersion: Graphite powder with a two-dimensional size of 30 micrometers is dispersed in alcohol with a volume fraction of 75% and subjected to ultrasonic treatment at a frequency of 10KHz~100KHz and an ultrasonic time of 30min~60min to form a uniform solution and obtain graphene dispersion. (3) Mixing aluminum powder dispersion and graphite dispersion: Mix aluminum powder dispersion and graphite dispersion, sonicate in water bath for 9 min at a frequency of 90 kHz, and then sonicate at a power of 200 W for 30 min to obtain graphite / aluminum powder mixed dispersion. (4) Oriented treatment and drying of graphite: The mixed dispersion obtained in step (3) is quick-frozen to form a mixture of aluminum, graphene and solid alcohol. The mixture is placed in a freeze dryer and dried at -100℃ for 36 hours to obtain oriented graphite / aluminum mixed powder.

[0049] The above method of filling the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder is as follows: the aluminum tube protective sleeve is inserted into the dried mixed powder at a 70°~90° angle relative to the vertical direction, and after filling with powder, the two ends of the aluminum tube protective sleeve are sealed.

[0050] The annealing process described above is performed in a vacuum or inert gas environment at a temperature of 300°C.

[0051] In the above drawing process, the drawing direction is along the axial direction of the aluminum tube protective sleeve, and the deformation of a single drawing is between 10% and 15%, finally obtaining a metal wire with a diameter ≤10mm.

[0052] Example 6 A graphene / aluminum composite conductor is composed of the following alloy components by mass percentage: 10.00% graphene, 0.03% Si, 0.03% Fe, with each of the remaining impurity elements ≤0.01%, and the balance being Al.

[0053] The preparation method of the aluminum-based composite material described above includes the following steps: First, fill the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder; second, axially pull the protective sleeve containing the mixed powder, and then anneal it in a vacuum or inert gas environment; then change the mold and pull it again, and anneal it again, and repeat the process.

[0054] The method for preparing the above-mentioned oriented graphite / aluminum mixed powder includes the following steps: (1) Preparation of aluminum powder dispersion: Disperse spherical aluminum powder with a particle size distribution of 80 mesh in 75% alcohol by volume, and perform ultrasonic treatment at a frequency of 100KHz for 60min to obtain aluminum powder dispersion. (2) Preparation of graphite dispersion: Graphite powder with a two-dimensional size of 10 micrometers is dispersed in alcohol with a volume fraction of 75% and subjected to ultrasonic treatment at a frequency of 100KHz for 60min to form a uniform solution and obtain graphene dispersion. (3) Mixing aluminum powder dispersion and graphite dispersion: Mix aluminum powder dispersion and graphite dispersion, sonicate in water bath for 10 min at a frequency of 100 kHz, and then sonicate at a power of 200 W for 30 min to obtain graphite / aluminum powder mixed dispersion. (4) Oriented treatment and drying of graphite: The mixed dispersion obtained in step (3) is quick-frozen to form a mixture of aluminum, graphene and solid alcohol. The mixture is placed in a freeze dryer and dried at -100℃ for 36 hours to obtain oriented graphite / aluminum mixed powder.

[0055] The above method of filling the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder is as follows: the aluminum tube protective sleeve is inserted into the dried mixed powder at a 70°~90° angle relative to the vertical direction, and after filling with powder, the two ends of the aluminum tube protective sleeve are sealed.

[0056] The annealing process described above is performed in a vacuum or inert gas environment at a temperature of 300°C.

[0057] In the above drawing process, the drawing direction is along the axial direction of the aluminum tube protective sleeve, and the deformation of a single drawing is between 10% and 15%, finally obtaining a metal wire with a diameter ≤10mm.

[0058] Table 1 shows the performance tests of the materials prepared in the comparative examples and the embodiments. The conductivity of the prepared materials was tested using a DDBJ-350 conductivity meter.

[0059] Table 1. Comparison of electrical conductivity of materials prepared in comparative examples and embodiments. Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.

Claims

1. A method for preparing a graphene / aluminum-based composite conductor, characterized in that, The composite conductor is composed of the following alloy components by mass percentage: graphene 1%-10%, Si ≤0.03%, Fe ≤0.03%, each of the remaining impurity elements ≤0.01%, and the balance being Al; The preparation method is as follows: First, a directionally arranged graphite / aluminum mixed powder is filled into an aluminum tube protective sleeve; second, the protective sleeve containing the mixed powder is directionally drawn, and then annealed in a vacuum or inert gas environment; then the mold is changed and the drawing is repeated, and the annealing is repeated to obtain a graphene / aluminum-based composite conductor. The preparation method of the oriented graphite / aluminum mixed powder includes the following steps: (1) Preparation of aluminum powder dispersion: Disperse spherical aluminum powder with a particle size distribution of 80-300 mesh in 75% alcohol by volume, and perform ultrasonic treatment to obtain aluminum powder dispersion; (2) Preparation of graphite dispersion: Disperse thin-layer graphite powder with a two-dimensional size of 10-100 micrometers in 75% alcohol by volume, and sonicate it to form a uniform solution to obtain graphite dispersion. (3) Mixing aluminum powder dispersion and graphite dispersion: Mix aluminum powder dispersion and graphite dispersion, and sonicate in a water bath for 5 to 10 minutes at a frequency of 10KHz~100KHz, and then sonicate at a power of 200W for 30 minutes to obtain graphite / aluminum powder mixed dispersion. (4) Oriented treatment and drying of graphite: After stopping the ultrasonic treatment, the mixed dispersion obtained in step (3) is immediately frozen using liquid nitrogen rapid cooling technology to form a mixture of aluminum, graphite and solid alcohol. The mixture is placed in a freeze dryer and dried at -100℃ for 24h~36h to obtain oriented graphite / aluminum mixed powder. The method of filling the aluminum tube protective sleeve with oriented graphite / aluminum mixed powder is as follows: the aluminum tube protective sleeve is inserted into the dried mixed powder at a 70°~90° angle relative to the vertical direction, and after filling with powder, the two ends of the aluminum tube protective sleeve are sealed.

2. The method for preparing the graphene / aluminum-based composite conductor according to claim 1, characterized in that, The annealing process takes place in a vacuum or inert gas environment at a temperature of 100℃ to 300℃.

3. The method for preparing the graphene / aluminum-based composite conductor according to claim 1, characterized in that, During the drawing process, the drawing direction is along the axial direction of the aluminum tube protective sleeve, and the deformation of a single drawing is between 10% and 15%, ultimately resulting in a metal wire with a diameter of ≤10mm.

4. The method for preparing the graphene / aluminum-based composite conductor according to claim 1, characterized in that, The frequency of ultrasonic treatment in steps (1) and (2) is 10KHz~100KHz, and the ultrasonic time is 30min~60min.

Citation Information

Patent Citations

  • High-strength high-conductivity graphene reinforced aluminum-based conductor wire and preparation method thereof

    CN115449672A

  • Electric conductor with graphene core and preparation method of electric conductor with graphene core

    CN106128545A

  • Carbon / metal composite material with microscopic orientation structure for electric contact and preparation method thereof

    CN108994300A

  • Graphene / aluminum-matrix composite for high-speed impact resistance and preparation method thereof

    CN109722556A