Aluminum alloy sheet for automobile chassis and method for manufacturing the same
Patent Information
- Application Number
- CN202410391994.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-02
AI Technical Summary
The production efficiency of existing aluminum alloy thin-walled structural parts is low, the forming difficulty is high, the mechanical properties are poor, and the poor fluidity of aluminum alloy melt in the traditional die casting process leads to difficulties in casting and many defects.
By introducing Zr into aluminum alloys to form Al₃Zr compounds to refine grains, optimizing chemical composition, controlling melting temperature and refining process, and employing vacuum die casting, combined with mold preheating and a reasonable filling speed, high-strength aluminum alloy thin sheets are prepared.
This technology enables one-time forming of high-strength aluminum alloy sheets without heat treatment, reducing production costs and energy consumption, improving production efficiency, reducing casting defects, and enhancing mechanical properties.
Smart Images

Figure CN118147496B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of die-cast aluminum sheet technology for automobiles, and more particularly to a method for manufacturing high-strength die-cast aluminum alloy thin sheets for automobile chassis. Background Technology
[0002] With the development of lightweighting in automobiles, replacing steel with aluminum has gradually become the mainstream in the automotive industry, attracting significant attention both domestically and internationally. The safety performance of a vehicle is largely influenced by its structural components, which are typically characterized by large dimensions and thin walls. Therefore, ensuring the mechanical properties of these structural components is crucial to guaranteeing vehicle safety.
[0003] Currently, aluminum alloy structural components require complex processing techniques such as rough rolling, precision rolling, sawing and washing, and even heat treatment during manufacturing. Processing aluminum alloys is difficult, energy-intensive, has a long production cycle, and low production efficiency.
[0004] CN112746202A discloses an aluminum alloy sheet and its manufacturing method. Based on the total amount of aluminum alloy, the sheet contains, by weight percentage, 1.4–1.5% Si, 0.1–0.4% Fe, 0–0.2% Cu, 0.03–0.17% Mn, 0.63–0.68% Mg, 0.1–0.15% Cr, 0.01–0.02% Ti, and 0–0.10% Zn, with the balance being Al. This manufacturing method improves the stamping formability and bake hardening properties of the alloy sheet. However, the method is relatively complex, requiring annealing and pre-aging treatment of the aluminum alloy, resulting in a long production cycle and low production efficiency.
[0005] It can be seen that existing technologies have optimized the element ratio and production process of aluminum alloy thin-walled structural parts to a certain extent, but there are still a series of problems such as low production efficiency. At the same time, when manufacturing aluminum alloy structural parts using the existing die casting process, the cooling rate is extremely fast and the fluidity of the aluminum alloy melt is poor, making it difficult for the melt to fill the mold, resulting in high difficulty in forming aluminum alloy structural parts and poor mechanical properties of the formed structural parts. Summary of the Invention
[0006] The main objective of this invention is to provide a method for obtaining high-strength aluminum alloy sheets through die casting, based on the application and development trends of aluminum alloy materials in automobiles. This invention features a simple manufacturing process, requires no heat treatment, and produces aluminum alloy sheets with excellent mechanical properties and low energy consumption, making them suitable for use in automotive chassis and meeting the requirements for lightweight automobiles.
[0007] To address the aforementioned problems, the first aspect of this invention provides a die-cast aluminum alloy, expressed as a weight percentage, wherein the chemical composition and mass percentage of the die-cast aluminum alloy are: Si: 0.20–0.50%, Fe: 0.40–0.60%, Cu: 3.00–4.40%, Mn: 0.55–1.15%, Mg: 2.00–2.90%, Cr: 0.02–0.04%, Zn: 0.20–0.30%, Ti: 0.03–0.06%, Zr: 0.15–0.20%, with the balance being Al.
[0008] In the aforementioned technical solution, by introducing the alloying element Zr into the aluminum alloy, it can react with aluminum to form Al3Zr compounds, which act as heterogeneous nucleation sites for aluminum grains, thereby significantly refining the grain size. Zr forms an active interface with aluminum at high temperatures, helping to reduce the formation of oxides and other impurities on the surface of the molten metal, thus reducing surface tension and effectively improving the fluidity of the high-temperature aluminum molten metal. Simultaneously, the introduction of Zr ensures sufficient feeding of the interdendritic liquid during solidification, thereby reducing the formation of voids and defects, significantly lowering the risk of crack formation, and thus enhancing the safety factor of automobiles. Although Zr exhibits a significant strengthening effect in aluminum alloys, excessive content may have negative effects. When the Zr content is too high, it may lead to the precipitation of a hard and brittle Zr5Al3 phase characterized by a close-packed hexagonal crystal structure within or between grains. Under significant stress, this phase may simultaneously induce transgranular fracture and intergranular fracture, significantly reducing the mechanical properties of the aluminum alloy. Therefore, rationally optimizing the Zr content is crucial for the design of future high-strength aluminum alloys. Compared with other rare earth elements such as Sc and Y, Zr has a comparable strengthening effect and is relatively cheaper. At the same time, it can make the high-temperature aluminum alloy melt have better fluidity, ensuring the formability of die-cast thin plates and effectively improving the mechanical properties of aluminum alloy thin plates at room temperature.
[0009] A second aspect of this invention provides a method for preparing die-cast aluminum alloy sheet for automobile chassis, the method comprising the following steps:
[0010] In one possible implementation, smelting is carried out: the intermediate alloy containing Zr is separately placed into a smelting furnace with aluminum ingots and aluminum alloy industrial waste for smelting. After ensuring that the two are smelted uniformly, they are mixed together. The smelting temperature in the furnace is controlled at 730-760℃. The smelting temperature of the aluminum liquid is not allowed to exceed 760℃ throughout the entire smelting process. During the aluminum alloy smelting process, the mixture is continuously stirred to remove slag and obtain the initial aluminum alloy liquid.
[0011] In the above technical solutions, separate melting is intended to ensure the uniformity of the alloy; strict control of the melting temperature in the furnace is intended to reduce hydrogen absorption and oxidation of the melt, reduce oxide content, control the melt structure, and ensure the mechanical properties of the die-cast aluminum alloy sheet; and strict control of the melting time in the furnace is intended to reduce the gas content of the melt, avoid continuous chemical reactions, and prevent deterioration of the melt structure.
[0012] In one possible implementation, refining and degassing are performed: the resulting molten aluminum alloy is transferred to a furnace for refining at a temperature of 725–750°C for 75–150 minutes. During this period, a mixture of nitrogen and chlorine is introduced for refining, with chlorine comprising approximately 3% of the total gas content and nitrogen flowing at a rate of 5–6.5 m³ / min. 3 / h, chlorine flow rate 0.1~0.25m 3 / h, the hydrogen content is controlled below 0.15ml / 100g Al, while the entrainment content is controlled below 0.20mm. 2 Within / kg, the final step involves removing the slag and letting it stand for 30-60 minutes, after which refining is complete.
[0013] In the above technical solution, nitrogen, chlorine and their products all have a refining effect, and can also decompose some aluminum oxide.
[0014] In one possible implementation, mold filling preparation is carried out: during the refining process, the metal die-casting mold is closed and locked, the gas in the pressure chamber and cavity of the die-casting mold is extracted, the mold is preheated to 150-200°C, and the aluminum alloy liquid is waited for filling.
[0015] In the above technical solution, preheating the mold can effectively reduce the thermal stress caused by rapid temperature changes during aluminum alloy die casting, thereby improving the fluidity of the aluminum alloy and reducing defects such as porosity and shrinkage. Furthermore, this approach also helps reduce the thermal stress on the mold, thus extending its service life.
[0016] In one possible implementation, die casting is performed: a certain amount of molten aluminum alloy is poured into the pressure chamber of the die casting machine, and the aluminum alloy is pumped into the metal mold at a filling speed of 34-42 m / s. The filling time is 0.040-0.060 s. After the die casting filling is completed, the pressure is held for 130-150 s. After the pressure holding is completed, the metal mold is unlocked and the casting is ejected to obtain an aluminum alloy sheet blank. The mold is then reset.
[0017] In the above technical solution, since the required average thickness of the casting is 4mm, the filling speed is selected as 34-42m / s and the filling time is selected as 0.040-0.060s based on experience and recommended values. Selecting this filling speed can not only improve the surface quality of the casting but also improve its mechanical properties. Selecting this filling time can avoid the formation of oxide slag in areas where air is not completely removed, thus improving the gradual molding effect.
[0018] In one possible implementation, post-processing of the blank is performed: the obtained aluminum alloy sheet blank is de-gated and flash is removed, and quality inspections are conducted on aspects such as structural integrity, dimensional compliance, and casting defects. The aluminum alloy sheet blank that meets the quality inspection standards undergoes post-processing, with all mating surfaces, contact surfaces, and various parts being polished smooth to a roughness Ra≤0.5μm.
[0019] Compared with existing technologies, the method for preparing die-cast aluminum alloy thin plates for automobile chassis proposed in this invention has the following advantages:
[0020] Compared with traditional automotive component manufacturing processes, this invention has a shorter process flow and lower manufacturing costs. It can form aluminum alloy sheets in one step without heat treatment, which greatly improves production efficiency and can obtain aluminum alloy sheets with higher yield strength, tensile strength and elongation.
[0021] 2. This invention employs vacuum die casting, effectively reducing defects such as porosity and pinholes in castings, minimizing surface blistering, and preventing severe deformation or even cracking in complex areas. It also addresses the drawbacks of traditional processes, such as the need for post-processing, high production costs, and long manufacturing cycles. Vacuum die casting significantly shortens the casting production cycle, improves casting quality, and reduces production costs.
[0022] 3. The present invention produces aluminum alloy thin sheets without heat treatment, reducing energy consumption during the heat treatment process, lowering manufacturing costs, and avoiding deformation of the aluminum alloy thin sheets during the heat treatment process.
[0023] 4. The die-cast aluminum alloy sheet for automobile chassis prepared using the technical solution of the present invention has high yield strength (greater than 250MPa) and tensile strength (greater than 300MPa), and high elongation (elongation ≥15%). Attached Figure Description
[0024] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments of this application will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 The graph shows a comparison of the yield strength, tensile strength, and elongation of Examples 2, 4, 6, Comparative Example 2, and Comparative Example 4. Detailed Implementation
[0026] The present invention will be further described below in conjunction with the implementation method.
[0027] Example 1:
[0028] The present invention relates to a die-cast aluminum alloy sheet for automotive chassis, expressed as a percentage by mass. The total chemical composition of the aluminum alloy sheet is as follows: Si: 0.251%, Fe: 0.453%, Cu: 3.413%, Mn: 0.674%, Mg: 2.859%, Cr: 0.027%, Zn: 0.218%, Ti: 0.038%, Zr: 0.152%, with the balance being Al.
[0029] Example 2:
[0030] Embodiment 1 of the present invention describes a method for preparing die-cast aluminum alloy thin plates for automobile chassis. The detailed steps of this method are as follows:
[0031] 1) Smelting: The intermediate alloy containing Zr is placed separately into the smelting furnace with aluminum ingots and aluminum alloy industrial waste for smelting. After ensuring that the two are smelted evenly, they are mixed together. The smelting temperature in the furnace is controlled at 735℃. The smelting temperature of the aluminum liquid is controlled within 760℃ throughout the smelting process. During the aluminum alloy smelting process, the mixture is continuously stirred to remove slag and obtain the initial aluminum alloy liquid.
[0032] 2) Refining and Degassing: The resulting molten aluminum alloy is transferred to a furnace for refining. The refining time is 75 minutes, and the refining temperature is 725℃. During this period, a mixture of nitrogen and chlorine gas is introduced for refining. The chlorine gas accounts for approximately 3% of the total gas content, and the nitrogen flow rate is 5.2 m³ / min. 3 / h, chlorine flow rate 0.18m 3 / h, the hydrogen content is controlled below 0.15ml / 100g Al, while the entrainment content is controlled below 0.20mm. 2 Within / kg, the final step involves removing the slag and letting it stand for 35 minutes to complete the refining process.
[0033] 3) Mold filling preparation: When refining is about to be completed, the metal die casting mold is closed and locked, the gas in the pressure chamber and cavity of the die casting mold is extracted, and the mold is preheated to 160°C to wait for the aluminum alloy liquid to fill the mold.
[0034] 4) Die casting: A certain amount of molten aluminum alloy is poured into the pressure chamber of the die casting machine. The aluminum alloy is pumped into the metal mold at a filling speed of 36m / s. The filling time is 0.042s. After the die casting filling is completed, the pressure is held for 130s. After the pressure holding is completed, the metal mold is unlocked and the casting is ejected to obtain an aluminum alloy sheet blank. The mold is then reset.
[0035] 5) Blank Post-processing: Remove the gate and flash from the obtained aluminum alloy sheet blanks, and conduct quality inspections on aspects such as structural integrity, dimensional compliance, and casting defects. The aluminum alloy sheet blanks that meet the quality inspection standards undergo post-processing, with all mating surfaces, contact surfaces, and other parts polished smooth to a roughness Ra≤0.5μm.
[0036] 6) Performance testing: The samples for room temperature tensile testing were processed according to GB / T 228.1-2021, and tensile tests were conducted on these materials on the WDW-100E universal tensile testing machine of Shandong Jianzhu University, with the tensile speed set to 1 mm / s.
[0037] Finally, the yield strength of the die-cast aluminum alloy sheet for automobile chassis prepared in Example 2 of the present invention is 268 MPa, the tensile strength is 335 MPa, and the elongation is ≥16.8%.
[0038] Example 3:
[0039] The present invention relates to a die-cast aluminum alloy sheet for automobile chassis, expressed as a percentage by mass. The total chemical composition of the aluminum alloy sheet is as follows: Si: 0.368%, Fe: 0.503%, Cu: 3.683%, Mn: 0.886%, Mg: 2.123%, Cr: 0.021%, Zn: 0.256%, Ti: 0.034%, Zr: 0.198%, with the balance being Al.
[0040] Example 4:
[0041] Embodiment 3 of the present invention describes a method for preparing die-cast aluminum alloy thin plates for automobile chassis. The detailed steps of this method are as follows:
[0042] 1) Smelting: The intermediate alloy containing Zr is placed separately into the smelting furnace with aluminum ingots and aluminum alloy industrial waste for smelting. After ensuring that the two are smelted evenly, they are mixed together. The smelting temperature in the furnace is controlled at 740℃. The smelting temperature of the aluminum liquid is controlled within 760℃ throughout the smelting process. During the aluminum alloy smelting process, the mixture is continuously stirred to remove slag and obtain the initial aluminum alloy liquid.
[0043] 2) Refining and Degassing: The obtained molten aluminum alloy is transferred to a furnace for refining. The refining time is 100 minutes, and the refining temperature is 730℃. During this period, a mixture of nitrogen and chlorine gas is introduced for refining. The chlorine gas accounts for approximately 3% of the total gas content, and the nitrogen flow rate is 5.5 m³ / min.3 / h, chlorine flow rate 0.20m 3 / h, the hydrogen content is controlled below 0.15ml / 100g Al, while the entrainment content is controlled below 0.20mm. 2 Within / kg, the final step involves removing the slag and letting it stand for 50 minutes to complete the refining process.
[0044] 3) Mold filling preparation: When refining is about to be completed, the metal die casting mold is closed and locked, the gas in the pressure chamber and cavity of the die casting mold is extracted, and the mold is preheated to 180°C to wait for the aluminum alloy liquid to fill the mold.
[0045] 4) Die casting: A certain amount of molten aluminum alloy is poured into the pressure chamber of the die casting machine. The aluminum alloy is pumped into the metal mold at a filling speed of 39 m / s. The filling time is 0.052 s. After the die casting filling is completed, the pressure is held for 140 s. After the pressure holding is completed, the metal mold is unlocked and the casting is ejected to obtain an aluminum alloy sheet blank. The mold is then reset.
[0046] 5) Blank Post-processing: Remove the gate and flash from the obtained aluminum alloy sheet blanks, and conduct quality inspections on aspects such as structural integrity, dimensional compliance, and casting defects. The aluminum alloy sheet blanks that meet the quality inspection standards undergo post-processing, with all mating surfaces, contact surfaces, and other parts polished smooth to a roughness Ra≤0.5μm.
[0047] 6) Performance testing: The samples for room temperature tensile testing were processed according to GB / T 228.1-2021, and tensile tests were conducted on these materials on the WDW-100E universal tensile testing machine of Shandong Jianzhu University, with the tensile speed set to 1 mm / s.
[0048] Finally, the yield strength of the die-cast aluminum alloy sheet for automobile chassis prepared in Example 4 of the present invention is 281 MPa, the tensile strength is 321 MPa, and the elongation is ≥17.9%.
[0049] Example 5:
[0050] The present invention relates to a die-cast aluminum alloy sheet for automotive chassis, expressed as a percentage by mass. The total chemical composition of the aluminum alloy sheet is as follows: Si: 0.429%, Fe: 0.532%, Cu: 4.231%, Mn: 1.008%, Mg: 2.413%, Cr: 0.036%, Zn: 0.267%, Ti: 0.052%, Zr: 0.183%, with the balance being Al.
[0051] Example 6:
[0052] Embodiment 5 of the present invention describes a method for preparing die-cast aluminum alloy thin plates for automobile chassis. The detailed steps of this method are as follows:
[0053] 1) Smelting: The intermediate alloy containing Zr is placed separately into the smelting furnace with aluminum ingots and aluminum alloy industrial waste for smelting. After ensuring that the two are smelted evenly, they are mixed together. The smelting temperature in the furnace is controlled at 755℃. The smelting temperature of the aluminum liquid is controlled within 760℃ throughout the smelting process. During the aluminum alloy smelting process, the mixture is continuously stirred to remove slag and obtain the initial aluminum alloy liquid.
[0054] 2) Refining and Degassing: The obtained molten aluminum alloy is transferred to a furnace for refining. The refining time is 135 minutes, and the refining temperature is 747℃. During this period, a mixture of nitrogen and chlorine gas is introduced for refining. The chlorine gas accounts for approximately 3% of the total gas content, and the nitrogen flow rate is 6.0 m³ / min. 3 / h, chlorine flow rate 0.21m 3 / h, the hydrogen content is controlled below 0.15ml / 100g Al, while the entrainment content is controlled below 0.20mm. 2 Within / kg, the final step involves removing the slag and letting it stand for 55 minutes, after which refining is complete.
[0055] 3) Mold filling preparation: When refining is about to be completed, the metal die casting mold is closed and locked, the gas in the pressure chamber and cavity of the die casting mold is extracted, and the mold is preheated to 190°C, waiting for the aluminum alloy liquid to fill the mold.
[0056] 4) Die casting: A certain amount of molten aluminum alloy is poured into the pressure chamber of the die casting machine. The aluminum alloy is pumped into the metal mold at a filling speed of 41 m / s. The filling time is 0.058 s. After the die casting filling is completed, the pressure is held for 150 s. After the pressure holding is completed, the metal mold is unlocked and the mold is separated. The casting is ejected to obtain an aluminum alloy sheet blank, and the mold is reset.
[0057] 5) Blank Post-processing: Remove the gate and flash from the obtained aluminum alloy sheet blanks, and conduct quality inspections on aspects such as structural integrity, dimensional compliance, and casting defects. The aluminum alloy sheet blanks that meet the quality inspection standards undergo post-processing, with all mating surfaces, contact surfaces, and other parts polished smooth to a roughness Ra≤0.5μm.
[0058] 6) Performance testing: The samples for room temperature tensile testing were processed according to GB / T 228.1-2021, and tensile tests were conducted on these materials on the WDW-100E universal tensile testing machine of Shandong Jianzhu University, with the tensile speed set to 1 mm / s.
[0059] Finally, the yield strength of the die-cast aluminum alloy sheet for automobile chassis prepared in Example 6 of the present invention is 285 MPa, the tensile strength is 352 MPa, and the elongation is ≥15.9%.
[0060] Comparative Example 1:
[0061] The present invention relates to a die-cast aluminum alloy sheet for automotive chassis, expressed as a percentage by mass. The total chemical composition of the aluminum alloy sheet is as follows: Si: 0.382%, Fe: 0.513%, Cu: 3.875%, Mn: 0.782%, Mg: 2.873%, Cr: 0.021%, Zn: 0.269%, Ti: 0.037%, Zr: 0.362%, with the balance being Al.
[0062] Comparative Example 2:
[0063] Comparative Example 1 of the present invention describes a method for preparing die-cast aluminum alloy sheet for automobile chassis. The detailed steps of this method are as follows:
[0064] 1) Smelting: The intermediate alloy containing Zr is placed separately into the smelting furnace with aluminum ingots and aluminum alloy industrial waste for smelting. After ensuring that the two are smelted evenly, they are mixed together. The smelting temperature in the furnace is controlled at 745℃. The smelting temperature of the aluminum liquid is controlled within 760℃ throughout the smelting process. During the aluminum alloy smelting process, the mixture is continuously stirred to remove slag and obtain the initial aluminum alloy liquid.
[0065] 2) Refining and Degassing: The resulting molten aluminum alloy is transferred to a furnace for refining. The refining time is 95 minutes, and the refining temperature is 738℃. During this period, a mixture of nitrogen and chlorine gas is introduced for refining. The chlorine gas accounts for approximately 3% of the total gas content, and the nitrogen flow rate is 6.5 m³ / min. 3 / h, chlorine flow rate 0.25m 3 / h, the hydrogen content is controlled within 0.15ml / 100g Al, and the impurity content is controlled within 0.20mm2 / kg. Finally, the slag is removed and the mixture is allowed to stand for 40 minutes. The refining is then complete.
[0066] 3) Mold filling preparation: When refining is about to be completed, the metal die casting mold is closed and locked, the gas in the pressure chamber and cavity of the die casting mold is extracted, and the mold is preheated to 200°C, waiting for the aluminum alloy liquid to fill the mold.
[0067] 4) Die casting: A certain amount of molten aluminum alloy is poured into the pressure chamber of the die casting machine. The aluminum alloy is pumped into the metal mold at a filling speed of 40m / s. The filling time is 0.052s. After the die casting filling is completed, the pressure is held for 150s. After the pressure holding is completed, the metal mold is unlocked and the mold is separated. The casting is ejected to obtain an aluminum alloy sheet blank, and the mold is reset.
[0068] 5) Blank Post-processing: Remove the gate and flash from the obtained aluminum alloy sheet blanks, and conduct quality inspections on aspects such as structural integrity, dimensional compliance, and casting defects. The aluminum alloy sheet blanks that meet the quality inspection standards undergo post-processing, with all mating surfaces, contact surfaces, and other parts polished smooth to a roughness Ra≤0.5μm.
[0069] 6) Performance testing: The samples for room temperature tensile testing were processed according to GB / T 228.1-2021, and tensile tests were conducted on these materials on the WDW-100E universal tensile testing machine of Shandong Jianzhu University, with the tensile speed set to 1 mm / s.
[0070] Ultimately, the die-cast aluminum alloy sheet for automobile chassis prepared in Comparative Example 2 of the present invention has a yield strength of 162 MPa, a tensile strength of 208 MPa, and an elongation of ≥7.3%.
[0071] Comparative Example 3:
[0072] The present invention relates to a die-cast aluminum alloy sheet for automobile chassis, expressed as a percentage by mass. The total chemical composition of the aluminum alloy sheet is as follows: Si: 0.361%, Fe: 0.509%, Cu: 3.898%, Mn: 0.798%, Mg: 2.846%, Cr: 0.021%, Zn: 0.296%, Ti: 0.055%, Zr: 0.037%, with the balance being Al.
[0073] Comparative Example 4:
[0074] Comparative Example 3 of the present invention describes a method for preparing die-cast aluminum alloy sheet for automobile chassis. The detailed steps of this method are as follows:
[0075] 1) Smelting: The intermediate alloy containing Zr is placed separately into the smelting furnace with aluminum ingots and aluminum alloy industrial waste for smelting. After ensuring that the two are smelted evenly, they are mixed together. The smelting temperature in the furnace is controlled at 745℃. The smelting temperature of the aluminum liquid is controlled within 760℃ throughout the smelting process. During the aluminum alloy smelting process, the mixture is continuously stirred to remove slag and obtain the initial aluminum alloy liquid.
[0076] 2) Refining and Degassing: The resulting molten aluminum alloy is transferred to a furnace for refining. The refining time is 95 minutes, and the refining temperature is 738℃. During this period, a mixture of nitrogen and chlorine gas is introduced for refining. The chlorine gas accounts for approximately 3% of the total gas content, and the nitrogen flow rate is 6.5 m³ / min. 3 / h, chlorine flow rate 0.25m 3 / h, the hydrogen content is controlled within 0.15ml / 100g Al, and the impurity content is controlled within 0.20mm2 / kg. Finally, the slag is removed and the mixture is allowed to stand for 40 minutes. The refining is then complete.
[0077] 3) Mold filling preparation: When refining is about to be completed, the metal die casting mold is closed and locked, the gas in the pressure chamber and cavity of the die casting mold is extracted, and the mold is preheated to 200°C, waiting for the aluminum alloy liquid to fill the mold.
[0078] 4) Die casting: A certain amount of molten aluminum alloy is poured into the pressure chamber of the die casting machine. The aluminum alloy is pumped into the metal mold at a filling speed of 40m / s. The filling time is 0.050s. After the die casting filling is completed, the pressure is held for 150s. After the pressure holding is completed, the metal mold is unlocked and the mold is separated. The casting is ejected to obtain an aluminum alloy sheet blank, and the mold is reset.
[0079] 5) Blank Post-processing: Remove the gate and flash from the obtained aluminum alloy sheet blanks, and conduct quality inspections on aspects such as structural integrity, dimensional compliance, and casting defects. The aluminum alloy sheet blanks that meet the quality inspection standards undergo post-processing, with all mating surfaces, contact surfaces, and other parts polished smooth to a roughness Ra≤0.5μm.
[0080] 6) Performance testing: The samples for room temperature tensile testing were processed according to GB / T 228.1-2021, and tensile tests were conducted on these materials on the WDW-100E universal tensile testing machine of Shandong Jianzhu University, with the tensile speed set to 1 mm / s.
[0081] Ultimately, the die-cast aluminum alloy sheet for automobile chassis prepared in Comparative Example 4 of the present invention has a yield strength of 132 MPa, a tensile strength of 196 MPa, and an elongation of ≥8.2%.
[0082] The specific embodiments of the present invention have been described above, but this is not intended to limit the scope of protection of the invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art without creative effort based on the technical solutions of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for preparing a die-cast aluminum alloy sheet for automobile chassis, characterized in that, It includes the following steps: The raw materials are prepared according to the alloy element composition of die-cast aluminum alloy sheet for automobile chassis, and then melted, refined, and degassed. The alloy element composition, by mass percentage, includes: Si: The aluminum alloy composition is as follows: 0.20–0.50%, Fe: 0.40–0.60%, Cu: 3.00–4.40%, Mn: 0.55–1.15%, Mg: 2.00–2.90%, Cr: 0.02–0.04%, Zn: 0.20–0.30%, Ti: 0.03–0.06%, Zr: 0.15–0.20%, other individual elements ≤0.050%, total amount of other impurity elements ≤0.100%, balance being Al; the aluminum alloy liquid is die-cast and the blank is post-processed to obtain die-cast aluminum alloy sheet for automobile chassis; The die casting process includes closing and locking the metal die casting mold, extracting gas from the pressure chamber and cavity of the die casting mold to achieve a vacuum state, preheating the mold to 150-200°C, pouring a certain amount of molten aluminum alloy into the pressure chamber of the die casting machine, pressing the molten aluminum alloy into the metal mold at a filling speed of 34-42 m / s, with a filling time of 0.040-0.060 s, holding the pressure for 130-150 s after the die casting filling is completed, unlocking the metal mold to separate the casting, ejecting the casting to obtain an aluminum alloy sheet blank, and resetting the mold.
2. The method for preparing die-cast aluminum alloy sheet for automobile chassis according to claim 1, characterized in that, The smelting process involves separately placing the Zr-containing intermediate alloy, aluminum ingots, and aluminum alloy industrial waste into a smelting furnace for smelting. The smelting temperature in the furnace is controlled at 730–760°C, and the smelting temperature of the molten aluminum is not allowed to exceed 760°C throughout the entire smelting process.
3. The method for preparing die-cast aluminum alloy sheet for automobile chassis according to claim 1, characterized in that, The refining process includes introducing a mixture of nitrogen and chlorine gases, with chlorine comprising 3% of the total gas content and nitrogen flowing at a rate of 5–6.5 m³ / h. 3 / h, chlorine flow rate 0.1~0.25m 3 / h, hydrogen content controlled within 0.15ml / 100g Al, and inclusion content controlled within 0.20mm. 2 For samples weighing less than 1 kg, the refining temperature is 725–750℃ and the refining time is 75–150 min. After refining, the slag is removed and the sample is allowed to stand for 30–60 min.
4. The method for preparing die-cast aluminum alloy sheet for automobile chassis according to claim 1, characterized in that, The post-processing of the blank includes removing the gate and flash, inspecting the blank for structural integrity, dimensional compliance, and casting defects, and polishing all mating surfaces, contact surfaces, and various parts of the aluminum alloy sheet blank that meet the quality inspection standards until the roughness Ra≤0.5μm.
5. A die-cast aluminum alloy sheet for automobile chassis, characterized in that, It is prepared by the method of die-cast aluminum alloy sheet for automobile chassis as described in any one of claims 1 to 4. The thickness of the die-cast aluminum alloy sheet for automobile chassis is 4.0±0.05mm, and it has a yield strength greater than 250MPa and a tensile strength greater than 300MPa, and an elongation of ≥15%.
Citation Information
Patent Citations
Aluminum alloy sheet for automobile body and production method thereof
CN112746202A
Zr-containing aluminum-alloy and homogenizing heat treatment method thereof
CN101168811A
Vacuum die casting method of aluminum alloy cylinders without cylinder sleeves
CN106756300A
High-toughness and high-fatigue-resistance aluminum alloy and preparation method thereof
CN115466889A