A method of ultrasonic peening a single crystal high temperature alloy surface and inhibiting recrystallization thereof
By forming an alloy layer on the surface of a single-crystal superalloy through ultrasonic shot peening alloying, the problem of recrystallization after shot peening of the single-crystal superalloy is solved, achieving efficient surface strengthening and recrystallization inhibition, and improving the high-temperature mechanical properties and service life of the single-crystal superalloy.
Patent Information
- Application Number
- CN202211555190.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Single-crystal superalloys are prone to recrystallization after shot peening. Existing methods for suppressing this recrystallization are complex and difficult to integrate efficiently with shot peening technology, which affects their high-temperature mechanical properties and service life.
Ultrasonic shot peening technology is used to alloy the surface of single-crystal high-temperature alloys. Metal powder, such as Al powder, is added into the ultrasonic shot peening chamber. The alloy layer is formed by repeated impact between the shot and the powder. Heat treatment is then used to suppress recrystallization.
This method achieves surface strengthening and recrystallization inhibition of single-crystal superalloys, improves surface properties, simplifies the process flow, and significantly enhances the high-temperature mechanical properties and service life of single-crystal superalloys.
Smart Images

Figure HDA0003983030330000011 
Figure HDA0003983030330000012 
Figure HDA0003983030330000021
Abstract
Description
Technical Field
[0001] This invention belongs to the field of surface treatment technology, and in particular relates to a method for strengthening the surface of single-crystal superalloys with ultrasonic shot peening and inhibiting their recrystallization. Background Technology
[0002] Nickel-based single-crystal superalloys are widely used as materials for advanced aero-engine blades and heavy-duty gas turbine blades due to their excellent high-temperature mechanical properties. However, during operation, these equipment inevitably suffer from start-up, shutdown, and vibration, which can easily cause fatigue damage to the blade tenons, limiting their further application in industry.
[0003] Surface shot peening is considered one of the most effective technologies for improving the fatigue performance and extending the service life of mechanical components. However, the high-temperature recovery and recrystallization problems after surface shot peening of single-crystal superalloys limit its development in this field. Currently, methods for suppressing recrystallization in single-crystal superalloys mainly include high-temperature recovery treatment, surface carburizing treatment, surface coating, and removal of surface deformation layers. However, these methods are mostly pre- or post-treatment processes before shot peening, making it difficult to effectively combine them with surface shot peening technology, and the recrystallization suppression effect of some methods is not significant.
[0004] Shot peening introduces large strain near the surface of single-crystal superalloys. During high-temperature service, this strain energy drives surface recovery and recrystallization, severely impairing their high-temperature mechanical properties. Therefore, the high-temperature recrystallization problem restricts the application of shot peening technology in the field of single-crystal superalloys. Existing methods for suppressing recrystallization involve complex equipment and cumbersome procedures, and are difficult to effectively combine with shot peening technology, resulting in significant limitations in engineering applications. Summary of the Invention
[0005] In view of this, the purpose of the present invention is to provide a method for ultrasonic shot peening to strengthen the surface of single-crystal superalloys and inhibit their recrystallization. The product obtained by the method provided by the present invention has good performance and can inhibit recrystallization.
[0006] This invention provides a method for ultrasonic shot peening to strengthen the surface of a single-crystal superalloy and inhibit its recrystallization, comprising:
[0007] The single-crystal high-temperature alloy is subjected to ultrasonic shot peening under the action of metal powder.
[0008] Preferably, the metal powder is Al powder.
[0009] Preferably, the particle size of the metal powder is 0.5 to 100 μm.
[0010] Preferably, the single-crystal superalloy is a nickel-based single-crystal superalloy, and the nickel content in the nickel-based single-crystal superalloy is 60-70 wt%.
[0011] Preferably, the ultrasonic shot peening treatment is performed in an ultrasonic shot peening chamber, which includes:
[0012] Ultrasonic shot peening chamber, ultrasonic shot peening chamber top cover, ultrasonic shot peening drive unit, vacuum pump and argon cylinder;
[0013] The ultrasonic shot peening chamber is a place for repeated impact between shot and metal powder and the sample.
[0014] The top cover of the ultrasonic shot peening chamber is used to fix the target material and is equipped with channels for adding metal powder, evacuating, and introducing Ar gas.
[0015] The ultrasonic shot peening drive unit is used to provide the power for repeated impacts of shot on the sample surface, and includes an ultrasonic generator, an ultrasonic transducer, an ultrasonic amplitude transformer, and an ultrasonic tool head.
[0016] Vacuum pumps are used for evacuating sealed cavities;
[0017] Argon cylinders are used for the input of Ar gas into sealed cavities.
[0018] Preferably, the metal powder is disposed in the cavity of the ultrasonic shot peening device, and the volume of the metal powder is 1 / 500 to 1 / 300 of the cavity volume.
[0019] Preferably, the shot peening process involves ultrasonically peening the pellets into ceramic pellets.
[0020] The diameter of the pellets is 1–4 mm;
[0021] The total projected area of the pellets on the ultrasonic tool head is 20-50% of the area of the ultrasonic tool head.
[0022] Preferably, the distance between the treated surface of the single-crystal high-temperature alloy and the ultrasonic tool head during the ultrasonic shot peening process is 5 to 20 mm.
[0023] Preferably, the ultrasonic working frequency in the ultrasonic shot peening process is 20-30 kHz, the working amplitude is 20-60 μm, and the ultrasonic shot peening time is 30-600 s.
[0024] Preferably, after the ultrasonic shot peening treatment is completed, the process further includes:
[0025] The obtained product is then subjected to heat treatment;
[0026] The heat treatment temperature is 1000–1300℃; the heat treatment time is 2–10 hours.
[0027] Ultrasonic shot peening is a novel shot peening strengthening technique that can generate shot peening intensity and residual compressive stress far exceeding those of traditional shot peening. Simultaneously, because the shot particles in ultrasonic shot peening equipment undergo random movement within a sealed cavity, if specific metal powder is added to the cavity, the shot particles, powder, and target material will undergo embedding, cold welding, and diffusion processes during repeated impacts, ultimately resulting in an alloy layer of a certain thickness on the target material surface. In this invention, during the ultrasonic shot peening process of single-crystal high-temperature alloys, surface alloying with Al powder, which can effectively inhibit recrystallization, can simultaneously achieve single-crystal surface strengthening and recrystallization suppression.
[0028] This invention proposes a method for strengthening the surface of single-crystal superalloys and inhibiting their recrystallization using an ultrasonic shot peening device. By rationally selecting the type of metal powder, powder volume, shot size and shot peening time, ultrasonic shot peening alloying treatment is performed on the single-crystal surface, which not only improves the surface properties of the single-crystal superalloy, but also inhibits the occurrence of recrystallization. Attached Figure Description
[0029] Figure 1 This is a schematic diagram of the ultrasonic shot peening and alloying cavity in an embodiment of the present invention;
[0030] Figure 2 The near-surface hardness distribution of the single-crystal superalloys treated in Example 1 and Comparative Example 1;
[0031] Figure 3 The XRD results of the surface of the single-crystal superalloy after treatment in Example 1 and Comparative Example 1 are shown.
[0032] Figure 4 The results are SEM and EDS of the single-crystal superalloy section after processing in Example 1.
[0033] Figure 5 The OM morphology of the single-crystal superalloy treated in Example 1 after non-vacuum heat treatment at 1250°C for 4 hours is shown.
[0034] Figure 6 The OM morphology of the single-crystal superalloy treated in Example 1 after vacuum heat treatment at 1250℃ for 4 hours;
[0035] Figure 7 The OM morphology of the single crystal superalloy treated in Comparative Example 1 after non-vacuum heat treatment at 1250℃ for 4 hours is shown.
[0036] Figure 8 The OM morphology of the single crystal superalloy treated in Comparative Example 1 after vacuum heat treatment at 1250℃ for 4 hours is shown.
[0037] Figure 9 The OM morphology of the single-crystal superalloy treated in Example 2 after non-vacuum heat treatment at 1250°C for 4 hours is shown.
[0038] Figure 10 The OM morphology of the single-crystal superalloy treated in Example 3 after non-vacuum heat treatment at 1250°C for 4 hours is shown. Detailed Implementation
[0039] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0040] This invention provides a method for ultrasonic shot peening to strengthen the surface of a single-crystal superalloy and inhibit its recrystallization, comprising:
[0041] The single-crystal high-temperature alloy is subjected to ultrasonic shot peening under the action of metal powder.
[0042] In this invention, the metal powder is preferably Al powder; the purity of the metal powder is preferably 99.9%; the particle size of the metal powder is preferably 0.5-100 μm, more preferably 1-90 μm, more preferably 5-80 μm, more preferably 10-70 μm, more preferably 20-60 μm, more preferably 30-50 μm, and most preferably 40 μm.
[0043] In this invention, the single-crystal superalloy is preferably a nickel-based single-crystal superalloy, and the nickel content in the nickel-based single-crystal superalloy is preferably 60-70 wt%, more preferably 65%. This invention does not impose any special restrictions on the composition of the nickel-based single-crystal superalloy; any nickel-based single-crystal superalloy composition well-known to those skilled in the art can be used, such as the composition disclosed in patent CN102732750B.
[0044] In this invention, the single-crystal high-temperature alloy is preferably a single-crystal high-temperature alloy that has undergone standard heat treatment.
[0045] In this invention, the single-crystal high-temperature alloy is preferably a single-crystal rod.
[0046] In this invention, it is preferable to perform surface treatment on the single-crystal superalloy to obtain a single-crystal sample with good surface quality, and then perform subsequent ultrasonic shot peening; the surface treatment preferably includes:
[0047] First, sand it with sandpaper, then polish it with machinery.
[0048] In this invention, the sandpaper grit used for sanding is preferably 150 to 2000#.
[0049] In this invention, the surface roughness after surface treatment is preferably 0.02 to 0.04 μm.
[0050] In this invention, the ultrasonic shot peening treatment is preferably performed in an ultrasonic shot peening cavity, such as... Figure 1 As shown, an ultrasonic shot peening cavity for ultrasonic shot peening and alloying of single-crystal high-temperature alloys, in conjunction with an ultrasonic shot peening device, has the functions of strengthening the material surface, preparing a surface alloy layer, isolating air, and preventing surface oxidation. Preferably, it includes: an ultrasonic shot peening cavity 1, an ultrasonic shot peening cavity top cover 2, an ultrasonic shot peening drive unit 3, a vacuum pump, and an argon gas cylinder, etc.; the ultrasonic shot peening cavity 1 is the place for repeated impact between shot and metal powder and the sample, preparing a strengthening layer and a surface alloy layer; the ultrasonic shot peening cavity top cover 2 is used to fix the target material and has channels for adding aluminum powder, evacuating, and introducing Ar gas; the ultrasonic shot peening drive unit 3 is used to provide the power for repeated impact of shot on the sample surface, and this unit includes an ultrasonic generator, an ultrasonic transducer, an ultrasonic amplitude transformer, and an ultrasonic tool head 4; the vacuum pump is used for evacuating the sealed cavity; and the argon gas cylinder is used for inputting Ar gas into the sealed cavity. The present invention does not impose any special limitations on the ultrasonic shot peening cavity used for ultrasonic shot peening and alloying of single crystal high-temperature alloys. Any cavity and related devices with ultrasonic shot peening apparatus known to those skilled in the art can be used. The diameter of the ultrasonic shot peening cavity is preferably 20-30 mm, more preferably 25 mm.
[0051] In this invention, it is preferable to fix the single-crystal high-temperature alloy sample on the top cover 2 of the ultrasonic shot peening cavity for ultrasonic shot peening treatment.
[0052] In this invention, the metal powder is preferably disposed in the cavity of the ultrasonic shot peening, and the volume of the metal powder is preferably 1 / 500 to 1 / 300 of the cavity volume, more preferably 1 / 450 to 1 / 350, and most preferably 1 / 400.
[0053] In this invention, it is preferable to open the feeding valve and feed Al powder 7 with a purity of 99.9% into the sealed cavity through the powder feeding port. The particle size of the Al powder is 0.5 to 100 μm, and the volume of the Al powder is 1 / 500 to 1 / 300 of the volume of the sealed cavity.
[0054] In this invention, the shot particles used for ultrasonic shot peening are preferably ceramic shot particles, more preferably zirconia shot particles and / or silicon nitride shot particles; the diameter of the shot particles is preferably 1-4 mm, more preferably 2-3 mm; the total projected area of the shot particles on the ultrasonic tool head is preferably 20-50% of the area of the ultrasonic tool head, more preferably 30-40%, and most preferably 35%.
[0055] In this invention, the distance between the treated surface of the single-crystal high-temperature alloy and the ultrasonic tool head during the ultrasonic shot peening process is preferably 5-20 mm, more preferably 10-15 mm, and most preferably 12-13 mm.
[0056] In this invention, it is preferable to add a certain number of zirconium oxide or silicon nitride ceramic pellets 6 with a diameter of Φ1 to 4 mm into the sealed cavity 1, and the total projected area of the pellets on the ultrasonic tool head 4 accounts for 20% to 50% of the tool head area; the distance between the high-temperature alloy treated surface and the tool head is adjusted to 5 to 20 mm.
[0057] In this invention, it is preferable to fix the top cover 2 of the ultrasonic shot peening cavity to the ultrasonic shot peening cavity 1 with screws, and seal the gap between them with a sealing ring.
[0058] In this invention, the ultrasonic shot peening process is preferably carried out under vacuum conditions, preferably by evacuating the sealed chamber with a vacuum pump to achieve a vacuum level of 8 to 12 Pa, more preferably 10 Pa.
[0059] In this invention, the ultrasonic shot peening process is preferably carried out under the protection of Ar gas; the purity of the Ar gas is preferably 99.9%; and the input rate of the Ar gas is preferably 0.5–1.5 L / cm. 3 More preferably, it is 0.8–1.2 L / cm³. 3 The optimal value is 1L / cm 3 The pressure of the Ar gas is preferably 0.05 to 0.15 MPa, more preferably 0.1 MPa.
[0060] In this invention, it is preferable to open the valve of the argon cylinder and introduce 99.9% pure Ar gas into the sealed cavity at an injection rate of 1 L / cm². 3 When the argon pressure in the sealed chamber rises to 0.1 MPa, stop feeding Ar gas and close the argon cylinder valve.
[0061] In this invention, the ultrasonic working frequency during the ultrasonic shot peening process is preferably 20-30 kHz, more preferably 23-27 kHz, and most preferably 25 kHz; the working amplitude is preferably 20-60 μm, more preferably 30-50 μm, and most preferably 40 μm; the ultrasonic shot peening time is preferably 30-600 s, more preferably 50-500 s, more preferably 100-400 s, and most preferably 200-300 s.
[0062] In this invention, it is preferable to turn on the ultrasonic shot peening drive unit 3 to perform ultrasonic shot peening and alloying treatment of single crystal high temperature alloy, with an ultrasonic working frequency of 20-30kHz, a working amplitude of 20-60μm for the tool head 4, and an ultrasonic shot peening time of 30-600s.
[0063] In this invention, a metal layer is formed on the surface of a single-crystal high-temperature alloy after ultrasonic shot peening. The metal layer is preferably an Al layer. The thickness of the metal layer is preferably 5-30 μm, more preferably 10-25 μm, and most preferably 15-20 μm.
[0064] In this invention, the ultrasonic shot peening treatment preferably further includes:
[0065] The resulting product is then subjected to heat treatment.
[0066] In this invention, the heat treatment temperature is preferably 1000–1300℃, more preferably 1050–1250℃, and most preferably 1100–1250℃; the heat treatment time is preferably 2–10 hours, more preferably 3–5 hours, and most preferably 4 hours; the heat treatment can be performed in a vacuum environment or a non-vacuum environment; the vacuum degree of the vacuum environment is preferably 10. -1 ~10 -3 Pa, more preferably 10 Pa -2 Pa.
[0067] In this invention, the method for ultrasonic shot peening to strengthen the surface of single-crystal superalloys and inhibit their recrystallization is as follows: Figure 1 As shown, preferably including:
[0068] The surface of the single-crystal high-temperature alloy sample 5 after standard heat treatment was polished with 150# to 2000# sandpaper and mechanically polished to obtain a single-crystal sample with good surface quality.
[0069] The above-mentioned single-crystal high-temperature alloy sample 5 was fixed to the top cover 2 of the ultrasonic shot peening cavity;
[0070] According to the actual shot peening requirements, a certain number of zirconium oxide or silicon nitride ceramic pellets 6 with a diameter of Φ1~4mm are added to the sealed cavity 1. The total projected area of the pellets on the ultrasonic tool head 4 accounts for 20%~50% of the tool head area; the distance between the high-temperature alloy treated surface and the tool head is adjusted to 5~20mm.
[0071] The top cover 2 of the ultrasonic shot peening chamber is fixed to the ultrasonic shot peening chamber 1 with screws, and the two are sealed with a sealing ring.
[0072] The sealed chamber was evacuated using a vacuum pump until the vacuum level reached 10 Pa.
[0073] Open the valve of the argon cylinder and introduce 99.9% pure Ar gas into the sealed cavity at a rate of 1 L / cm². 3 When the argon pressure in the sealed chamber rises to 0.1 MPa, stop feeding Ar gas and close the argon cylinder valve.
[0074] Open the feeding valve and feed Al powder 7 with a purity of 99.9% into the sealed cavity through the powder feeding port. The particle size of Al powder is 0.5-100μm and the volume of Al powder is 1 / 500-1 / 300 of the volume of the sealed cavity.
[0075] Turn on the ultrasonic shot peening drive unit 3 to perform ultrasonic shot peening and alloying treatment of single crystal high temperature alloy. The ultrasonic working frequency is 20-30kHz, the working amplitude of the tool head 4 is 20-60μm, and the ultrasonic shot peening time is 30-600s.
[0076] After the above ultrasonic shot peening alloying treatment, an Al metal layer 8 with a thickness of 5 to 30 μm can be prepared on the surface of a single crystal high-temperature alloy.
[0077] This invention proposes a method for strengthening the surface of single-crystal superalloys and inhibiting their recrystallization using ultrasonic shot peening. Single-crystal superalloys are selected as the research object. Al powder is added during the ultrasonic shot peening process. Through high strain rate deformation and deformation-induced diffusion process, an Al metal layer is prepared on the surface of the single-crystal superalloy, thereby achieving the purpose of strengthening the single-crystal surface and inhibiting its recrystallization.
[0078] This invention proposes a method for strengthening the surface of single-crystal superalloys and inhibiting recrystallization using ultrasonic shot peening. This method overcomes the recrystallization problem that occurs after traditional shot peening of single-crystal superalloys, achieving both surface strengthening and high-temperature recrystallization inhibition in a single step. Furthermore, this method overcomes the problems of existing recrystallization inhibition methods being cumbersome, inefficient, and unable to be effectively combined with shot peening technology. The method provided by this invention is simple, provides accurate and detailed measurements, and achieves a strengthening effect comparable to that of ultrasonic shot peening alone. The prepared alloy layer is uniform and dense, and recrystallization inhibition is significant after high-temperature annealing. It is an ideal method for strengthening and inhibiting recrystallization of single-crystal superalloys, and is of great significance for further expanding the application of ultrasonic shot peening technology in the field of single-crystal superalloys.
[0079] The DD33 single crystal rods used in the following embodiments of the present invention were prepared according to Example 1 of Chinese Patent CN102732750B.
[0080] Example 1
[0081] The experimental material used was a third-generation single-crystal high-temperature alloy DD33 single crystal rod with
[001] orientation. After the single crystal rod was subjected to standard heat treatment (1335℃ / 10h, air cooling; 1150℃ / 4h, air cooling; 870℃ / 24h, air cooling), a circular test block with a thickness of 5mm was taken along the (001) surface using a wire cutting machine. The (001) surface was then ground and polished to obtain a surface with a surface roughness of Ra0.03μm.
[0082] The single crystal sample is fixed on the top cover of the ultrasonic shot peening chamber; Φ3mm zirconia pellets are added to the Φ25mm diameter chamber, and the total projected area of the pellets on the workpiece head accounts for 40% of the tool head area; the distance between the sample treatment surface and the tool head is adjusted to 10mm, and the top cover is fixed on the ultrasonic shot peening chamber.
[0083] Turn on the vacuum pump to maintain the vacuum level of the cavity at 10 Pa; introduce Ar gas into the cavity to bring the pressure inside the cavity to 0.1 MPa.
[0084] Open the feeding valve and feed 99.9% pure Al powder into the sealed cavity through the powder feeding port. The Al powder particle size is 1μm and the volume of Al powder is 1 / 400 of the volume of the sealed cavity.
[0085] The ultrasonic shot peening drive unit is activated to perform ultrasonic shot peening strengthening and alloying treatment of single crystal high temperature alloy. The ultrasonic working frequency is 20kHz, the working amplitude of the tool head is 30μm, and the ultrasonic shot peening time is 300s.
[0086] Comparative Example 1
[0087] The ultrasonic shot peening treatment was performed according to the method of Example 1, except that the Al powder feeding step was not performed.
[0088] Example 2
[0089] The ultrasonic shot peening treatment was performed according to the method of Example 1, except that the Al powder in Example 1 was replaced with W (tungsten) powder.
[0090] Example 3
[0091] The ultrasonic shot peening treatment was performed according to the method of Example 1, except that the Al powder in Example 1 was replaced with C (carbon) powder.
[0092] Performance testing
[0093] The products prepared in the examples were observed and tested using a microhardness tester, XRD, and SEM.
[0094] The DD33 samples treated in Example 1 and Comparative Example 1 were tested for hardness in the depth direction using a microhardness tester. The results are as follows: Figure 2 As shown, it can be seen that the samples treated with ultrasonic shot peening alloying (Example 1) and ultrasonic shot peening strengthening (Comparative Example 1) can form a work-hardened layer with a depth of 250-300 μm near the surface, and there is no significant difference in the hardness distribution. This indicates that ultrasonic shot peening alloying can achieve the same surface strengthening effect as ultrasonic shot peening strengthening.
[0095] Figure 3The XRD curves of the single-crystal high-temperature alloy surfaces after treatment in Example 1 and Comparative Example 1 of the present invention show that the single-crystal surface after treatment in Example 1 not only has Ni3Al peaks but also Al powder, indicating that an Al metal layer has been formed on the surface of the sample; while the single-crystal surface after treatment in Comparative Example 1 only has Ni3Al peaks, indicating that no alloy layer has been formed on the surface of the sample.
[0096] Figure 4 The SEM and EDS results of the single-crystal high-temperature alloy cross section after processing in Example 1 of the present invention show that a dense Al metal layer with an average thickness of about 10 μm can be prepared on the single crystal surface after processing in Example 1, indicating that the present invention can realize the surface alloying of materials.
[0097] The single-crystal superalloy sample treated in the examples was placed at 1250°C and subjected to non-vacuum or vacuum conditions (vacuum degree of 10). -3 The sample was kept at a constant temperature (Pa) for 4 hours, and recrystallization was examined using an optical microscope (OM). OM images of the sample treated in Example 1 under non-vacuum and vacuum conditions are shown below. Figure 5 and Figure 6 As shown; OM images of the processed sample in non-vacuum and vacuum environments are shown in Comparative Example 1. Figure 7 and Figure 8 As shown; OM images of the samples treated in Examples 2 and 3 after heat treatment in a non-vacuum environment are shown below. Figure 9 and Figure 10 As shown; it can be seen that, regardless of whether it is non-vacuum or vacuum heat treatment, recrystallization occurs only in a very small area near the surface of the sample treated in Example 1; while in Comparative Example 1, after non-vacuum heat treatment, a completely recrystallized layer of about 50 μm thickness is formed on the surface. Figure 7 After vacuum heat treatment, a fully recrystallized layer of approximately 20 μm thickness and a cellular recrystallized layer of approximately 100 μm thickness are formed on the surface. Figure 8 In Examples 2 and 3, significant surface recrystallization layers and cellular recrystallization layers also formed on the surface after non-vacuum heat treatment. The above experimental results demonstrate that the present invention can significantly suppress the formation of fully recrystallized layers and cellular recrystallized layers in single-crystal alloys.
[0098] This invention overcomes the recrystallization problem of single crystals after traditional shot peening during high-temperature service. It innovatively applies ultrasonic shot peening surface alloying technology to the field of single-crystal superalloys, achieving surface strengthening and recrystallization suppression in a single-step process. This invention overcomes the problems of existing recrystallization suppression methods being cumbersome, inefficient, and unable to be effectively combined with shot peening technology. The equipment is simple, the operation is convenient, and a single treatment time does not exceed 10 minutes. After treatment, the near-surface hardness of the single crystal is significantly improved, and recrystallization is significantly suppressed. This invention can achieve highly efficient surface strengthening and recrystallization suppression of single-crystal superalloys.
[0099] While the invention has been described and illustrated with reference to specific embodiments thereof, such description and illustration are not intended to limit the invention. It will be readily understood by those skilled in the art that various changes may be made to suit particular circumstances, materials, compositions, substances, methods, or processes to the objectives, spirit, and scope of this application without departing from the true spirit and scope of the invention as defined by the appended claims. All such modifications are intended to be within the scope of the appended claims. Although the methods disclosed herein have been described with reference to specific operations performed in a particular order, it should be understood that these operations may be combined, subdivided, or reordered to form equivalent methods without departing from the teachings of the invention. Therefore, unless specifically indicated herein, the order and grouping of operations are not a limitation of this application.
Claims
1. A method for ultrasonic shot peening to strengthen the surface of a single-crystal superalloy and inhibit its recrystallization, comprising: The single-crystal high-temperature alloy is subjected to ultrasonic shot peening under the action of metal powder; The metal powder is Al powder; the single-crystal high-temperature alloy is a nickel-based single-crystal high-temperature alloy. The ultrasonic shot peening process is carried out in an ultrasonic shot peening chamber, which includes a vacuum pump for evacuating the sealed chamber. The distance between the treated surface of the single-crystal high-temperature alloy and the ultrasonic tool head during the ultrasonic shot peening process is 5~20mm; the ultrasonic working frequency during the ultrasonic shot peening process is 20~30KHz, the working amplitude is 20~60μm, and the ultrasonic shot peening time is 30~600s.
2. The method according to claim 1, characterized in that, The particle size of the metal powder is 0.5~100μm.
3. The method according to claim 1, characterized in that, The nickel content in the nickel-based single-crystal superalloy is 60~70wt%.
4. The method according to claim 1, characterized in that, The ultrasonic shot peening process is performed in an ultrasonic shot peening chamber, which further includes: Ultrasonic shot peening chamber, ultrasonic shot peening chamber top cover, ultrasonic shot peening drive unit and argon gas cylinder. The ultrasonic shot peening chamber is a place for repeated impact between shot and metal powder and the sample. The top cover of the ultrasonic shot peening chamber is used to fix the target material and is equipped with channels for adding metal powder, evacuating, and introducing Ar gas. The ultrasonic shot peening drive unit is used to provide the power for repeated impacts of shot on the sample surface, and includes an ultrasonic generator, an ultrasonic transducer, an ultrasonic amplitude transformer, and an ultrasonic tool head. Argon cylinders are used for the input of Ar gas into sealed cavities.
5. The method according to claim 1, characterized in that, The metal powder is placed in the cavity of the ultrasonic shot peening device, and the volume of the metal powder is 1 / 500 to 1 / 300 of the cavity volume.
6. The method according to claim 1, characterized in that, The shot peening process used in the ultrasonic shot peening is ceramic shot. The diameter of the pellets is 1~4mm; The total projected area of the pellets on the ultrasonic tool head is 20-50% of the area of the ultrasonic tool head.
7. The method according to claim 1, characterized in that, The ultrasonic shot peening process, after completion, also includes: The obtained product is then subjected to heat treatment; The heat treatment temperature is 1000~1300℃; the heat treatment time is 2~10h.
Citation Information
Patent Citations
Nickel base single crystal superalloy with low cost and low density
CN102732750B
Metal surface alloying method based on ultrasonic shot-peening and application thereof
CN102851663A