Low driving potential Zn-Mn-X alloy sacrificial anode and preparation method thereof

By preparing Zn-Mn-X alloy sacrificial anodes, the problem of low current efficiency of aluminum alloy anodes in deep-sea environments was solved, achieving high-efficiency high-strength steel cathodic protection suitable for all marine environments, avoiding hydrogen embrittlement and reducing costs.

CN118147648BActive Publication Date: 2026-11-20CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410246323.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-05
Publication Date
2026-11-20
Estimated Expiration
2044-03-05

AI Technical Summary

Technical Problem

Existing aluminum alloy sacrificial anodes have low current efficiency in extreme marine environments such as deep sea, and cannot effectively avoid hydrogen embrittlement of high-strength steel materials. Furthermore, existing low drive potential anodes are not suitable for operating potentials in alternating wet and dry environments.

Method used

Based on Zn-Mn-X alloy, high-potential alloying elements such as Ga, Sn, Pb, and Sb are added to prepare low-driving-potential Zn-Mn-X alloy sacrificial anodes through metallurgical processes. This increases the working potential to -0.75 to -0.94V, achieves a current efficiency of over 90%, and has micron-sized high-potential precipitates distributed at grain boundaries and within grains, reducing crusting and improving activity.

Benefits of technology

It achieves efficient cathodic protection for high-strength steel in all marine environments, significantly improves current efficiency, avoids hydrogen embrittlement, is suitable for deep-sea and polar environments, and reduces processing costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004726037380000031
    Figure BDA0004726037380000031
  • Figure BDA0004726037380000041
    Figure BDA0004726037380000041
  • Figure BDA0004726037380000051
    Figure BDA0004726037380000051
Patent Text Reader

Abstract

The application belongs to the technical field of metal material corrosion protection, and particularly relates to a Zn-Mn-X alloy sacrificial anode with low driving potential, high activity and high current efficiency in full-sea marine environment, and capable of avoiding hydrogen embrittlement of high-strength steel materials, and a preparation method thereof. The sacrificial anode is a zinc alloy sacrificial anode, and its components include Zn, Mn and high-potential alloying element X. Different from an aluminum alloy anode, the surface corrosion layer is mainly ZnO / Zn(OH)2, and the structure is loose and porous, and the crust is poor, so that the activation capacity of the anode can be more easily ensured, and the current efficiency is above 90%, which is significantly higher than 75% to 86.5% of the aluminum alloy anode, and has higher activity, and is particularly suitable for cathodic protection of high-strength steel in deep-sea and polar environments. Meanwhile, the smelting preparation process is a three-stage feeding mode matched with different melting point metals, the smelting temperature of the zinc alloy is 550 to 700 DEG C, which is lower than the smelting temperature of the aluminum alloy, and no heat treatment is needed, so that the smelting energy consumption is small, and the processing cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical fields:

[0001] This invention belongs to the field of metal material corrosion protection technology, specifically relating to a Zn-Mn-X alloy sacrificial anode with low driving potential, high activity and high current efficiency in marine environments across the entire ocean, and capable of preventing hydrogen embrittlement of high-strength steel materials, as well as its preparation method. Background technology:

[0002] High-strength steel, with its high specific strength, is widely used in the fabrication of structural materials for marine equipment. However, high-strength steel structures are subject to long-term corrosion from seawater during service, necessitating reasonable and effective cathodic protection measures. Previous research indicates that the appropriate cathodic protection potential range for 785–980 MPa grade high-strength steel used in marine equipment should be -0.78 to -0.94 V (vs. Ag / AgCl). However, the current operating potential of sacrificial anodes used in underwater equipment, at -1.05 to -1.12 V, poses a risk of hydrogen embrittlement to high-strength steel. In practice, to avoid hydrogen embrittlement during use, the operating potential of sacrificial anodes should be between -0.75 and -0.94 V under normal conditions, and between -0.70 and -0.94 V under alternating wet and dry conditions.

[0003] In existing technologies, low-drive-potential sacrificial anodes for seawater are mainly aluminum alloy sacrificial anodes, which significantly improve the potential, but the overall current efficiency is below 86.5%, ranging from 75% to 86%, making them unsuitable for long-term service in extreme marine environments such as deep seas. For example, Chinese Patent 202211537872.2 discloses a low-drive-potential aluminum alloy sacrificial anode for seawater cooling systems, comprising a sacrificial anode body and a core. The core is encapsulated within the sacrificial anode body. The sacrificial anode body is primarily composed of aluminum, with added gallium, tin, antimony, and copper. The weight percentages of each component are: gallium 0.3%–0.5%, tin 0.01%–0.1%, antimony 0.005%–0.02%, copper 0.01%–0.1%, iron impurities ≤0.06%, and the balance being aluminum. Its operating potential is -0.75V to -0.90V, and its current efficiency is 75%–79.5%. Chinese Patent 200810249622.2 discloses a low-drive-potential aluminum alloy sacrificial anode, which uses high-purity aluminum as the main raw material and adds zinc, gallium, and silicon. The weight percentages of each component are: zinc 0.05-1.0%, gallium 0.05-0.3%, silicon 0.5-1.5%, and other impurities iron + copper + nickel ≤0.15%, calcium ≤0.15%, with the balance being aluminum. Its working potential is -0.80V to -0.85V, and its current efficiency is 85.1% to 86.2%. Chinese Patent 201610136266.8 discloses a low-drive-potential aluminum alloy sacrificial anode material, which, by weight percentage, contains 0.5-1% zinc (Zn), 0.018-0.05% indium (In), 0.1-0.4% silicon (Si), 0.1-1% cerium (Ce), and the balance is aluminum (grade Al99.85). The impurities are controlled to be ≤0.12% iron (Fe) and ≤0.01% copper (Cu). Its working potential is -0.77V to -0.85V, and its current efficiency is 85.01% to 86.12%. Chinese Patent 201910417732.3 discloses a low-drive-potential aluminum alloy sacrificial anode suitable for seawater, comprising the following raw materials by weight percentage: aluminum 85%-90%, zinc 2%-5%, bismuth 1%-3%, manganese 0.05%-0.08%, and gallium 0.02%-0.04%; its operating potential is -0.81 to -0.87V, and its current efficiency is 83% to 86%. Therefore, a method for preparing a highly active, low-potential anode using a zinc alloy sacrificial anode with higher current efficiency is being developed for use in high-strength steel cathodic protection of full-ocean-depth marine equipment. Summary of the Invention:

[0004] The purpose of this invention is to overcome the shortcomings of existing technologies and to develop a low-driving-potential Zn-Mn-X alloy sacrificial anode and its preparation method. Based on Zn-Mn alloy, alloying elements with potentials higher than zinc (-1.03V), such as Ga (-0.97V), Sn (-0.38V), Pb (-0.40V), and Sb (-0.09V), are added to prepare a zinc alloy high-activity low-potential anode, which increases the protection potential to -0.75 to -0.94V and achieves a current efficiency of over 90%.

[0005] To achieve the above objectives, the low-driving-potential Zn-Mn-X alloy sacrificial anode of the present invention is prepared by metallurgical or smelting processes. Its composition includes Zn, Mn, and a high-potential alloying element X. The content of Mn is 0.5–2.0 wt%, the content of X is ≤2 wt%, and the balance is Zn. X is one or more of Ga, Sn, Pb, and Sb, with the content of Ga being 0.01–1.9 wt%, and the contents of Sn, Pb, and Sb each being 0.01–1 wt%. The content of impurities (Fe) is...

[0006] <0.03wt%.

[0007] The process of preparing the low-driving-potential Zn-Mn-X alloy sacrificial anode according to the present invention is as follows:

[0008] First, heat the pure zinc to 550–700°C to molten state;

[0009] Then, add the Zn-Mn master alloy and mix thoroughly.

[0010] Finally, the temperature was lowered to 500℃, and one or more of the low-melting-point Ga, Sn, Pb, and Sb were added to the melt. After thorough stirring, the melt was held at a casting temperature of 430–500℃ for 4–8 minutes to obtain a Zn-Mn-X alloy sacrificial anode with an average grain size of less than 500 μm. The potential is 160–290 mV higher than that of the zinc matrix. The working potential in seawater is -0.75V to -0.94V, the current efficiency is ≥90%, the surface dissolution is uniform, and the corrosion products are easily detached. The micron-sized high-potential precipitate (Mn(Zn,Ga)) formed by the low-melting-point alloying elements... 13 The phases (Sn, Zn3Sb2, Pd3Mn2, and PdZn) are distributed at grain boundaries and within grains, which can increase the working potential, reduce the driving potential, and pierce the corrosion product layer. They also reduce crusting and increase activity, making them suitable for cathodic protection of high-strength steel structures in all marine environments. Among them, Mn(Zn,Ga) 13 The grain sizes of the Sn, Zn3Sb2, Pd3Mn2 and PdZn phases are all 20–50 μm.

[0011] Compared with existing technologies, the sacrificial anode of this invention is a zinc alloy sacrificial anode, which differs from aluminum alloy anodes. The surface corrosion layer is mainly ZnO / Zn(OH)2, with a loose and porous structure and poor crusting, making it easier to ensure the activation capacity of the anode. Furthermore, the current efficiency is above 90%, significantly higher than the 75% to 86.5% of aluminum alloy anodes, exhibiting higher activity. It is particularly suitable for cathodic protection of high-strength steel in deep-sea and polar environments. At the same time, the smelting and preparation process adopts a three-stage feeding method to accommodate metals with different melting points. The smelting temperature of zinc alloy is 550 to 700°C, lower than the smelting temperature of aluminum alloy (680 to 800°C). X is a low-melting-point metal element, requiring no heat treatment, resulting in low smelting energy consumption and low processing costs. Attached image description:

[0012] Figure 1 Metallographic image of the low-driving-potential Zn-Mn-X alloy sacrificial anode prepared in Example 1 of this invention.

[0013] Figure 2 A photograph of the corroded surface of the low-driving-potential Zn-Mn-X alloy sacrificial anode (serial number 1) prepared in Example 1 of this invention. Specific implementation methods:

[0014] The present invention will be further described below with reference to the accompanying drawings and specific implementation methods.

[0015] Example 1:

[0016] The mass percentages of each element in the low-driving-potential Zn-Mn-X alloy sacrificial anode involved in this embodiment are shown in Table 1:

[0017]

[0018]

[0019] Wherein, X is one of Ga, Sn, Pb, and Sb, with the balance being Zn; among them, Ga element can improve the surface activity of the alloy by reduction deposition on the metal surface, and can also refine the alloy structure to a certain extent, improve its uniform corrosion ability and electrical properties, and the maximum room temperature solubility of Ga element in zinc alloy is 1.9% (at), which meets the conditions for activation on the zinc alloy surface; the standard electrode potential of Sn element is -0.38V; the standard electrode potential of Pb element is -0.13V, and the solubility in zinc liquid at a temperature of 450℃ can reach up to 1.5%; the standard electrode potential of Sb element is -0.24V, which can lower the melting point of zinc in zinc liquid, improve the fluidity of zinc liquid during casting, improve the density of zinc plating layer, inhibit grain boundary corrosion, and improve the corrosion uniformity of zinc alloy anode.

[0020] The method for preparing the low-driving-potential Zn-Mn-X alloy sacrificial anode in this embodiment involves placing high-purity Zn, low-melting-point alloying element X, and intermediate alloy into a resistance melting furnace for melting according to their melting points. The specific process is as follows:

[0021] First, heat the pure zinc to 550–700°C to molten state;

[0022] Then, add the Zn-Mn master alloy and mix thoroughly.

[0023] Finally, the temperature is lowered to 500℃, and one of the low-melting-point Ga, Sn, Pb, and Sb is added to the melt. After thorough stirring with a graphite rod or a stirring device, the melt is held at a casting temperature of 430–500℃ for 4–8 minutes to obtain a Zn-Mn-X alloy sacrificial anode ingot. The scanning electron microscope image of the microstructure of the low-driving-potential Zn-Mn-X alloy sacrificial anode (serial number 1) is shown below. Figure 1 As shown, the alloy grain size of the low driving potential Zn-Mn-X alloy sacrificial anodes in serial numbers 1-4 is 100-500 μm. The alloying element-rich precipitates mainly precipitate at the grain boundaries, with a small amount distributed within the grains. The size of the precipitates is less than 100 μm.

[0024] Accelerated testing of the electrochemical performance of sacrificial anodes was conducted according to national standard GB / T 17848-1999. The test results of the low-driving-potential Zn-Mn-X alloy sacrificial anode (serial number 1) in seawater at room temperature are as follows: Figure 2 As shown, its operating potential is -0.85 to -0.94V, its current efficiency is 90.1% to 95.2%, there is no obvious adhesion of corrosion products, and the anodic dissolution is uniform with no obvious local corrosion.

[0025] Example 2:

[0026] The mass percentages of each element in the low-driving-potential Zn-Mn-X alloy sacrificial anode involved in this embodiment are shown in Table 2:

[0027]

[0028] Wherein, the element X is any two of Ga, Sn, Pb, and Sb, and the balance is Zn; the preparation method refers to the preparation method involved in Example 1.

[0029] Accelerated testing of the electrochemical performance of sacrificial anodes was conducted according to the national standard GB / T 17848-1999. The test results of the low driving potential Zn-Mn-X alloy sacrificial anodes (serial number 5-11) in seawater at room temperature were obtained. The working potential was -0.80 to -0.94V, the current efficiency was 92.1% to 96.4%, the corrosion products showed no obvious adhesion, and the anode dissolved uniformly without obvious local corrosion.

[0030] Example 3:

[0031] The mass percentages of each element in the low-driving-potential Zn-Mn-X alloy sacrificial anode involved in this embodiment are shown in Table 3:

[0032]

[0033]

[0034] Wherein, the X element is any three of Ga, Sn, Pb, and Sb, with the balance being Zn; the preparation method refers to the preparation method involved in Example 1.

[0035] Accelerated testing of the electrochemical performance of sacrificial anodes was conducted according to the national standard GB / T 17848-1999. The test results of the low driving potential Zn-Mn-X alloy sacrificial anode (serial number 12-21) in seawater at room temperature were obtained. The working potential was -0.75 to -0.94 V, the current efficiency was 95.1% to 97.3%, no obvious corrosion products were attached, and the anode dissolved uniformly without obvious local corrosion.

[0036] Example 4:

[0037] The mass percentages of each element in the low-driving-potential Zn-Mn-X alloy sacrificial anode involved in this embodiment are shown in Table 4:

[0038]

[0039] Wherein, the element X is Ga, Sn, Pb and Sb, and the balance is Zn; the preparation method is the same as that described in Example 1.

[0040] Accelerated testing of the electrochemical performance of sacrificial anodes was conducted according to the national standard GB / T 17848-1999. The test results of the low driving potential Zn-Mn-X alloy sacrificial anodes (serial numbers 22-24) in seawater at room temperature were obtained. The working potential was -0.75 to -0.90 V, the current efficiency was 96.7% to 98.6%, the corrosion products showed no obvious adhesion, and the anode dissolved uniformly without obvious local corrosion.

Claims

1. A low-driving-potential Zn-Mn-X alloy sacrificial anode, prepared by a melting process, characterized in that, The components include Zn, Mn and a low-melting-point alloying element X, where X is one or more of Ga, Sn, Pb and Sb; The content of Ga is 0.01–1.9 wt%, the content of Sn, Pb and Sb is 0.01–1 wt%, the content of impurities is <0.03 wt%, the content of Mn is 0.5–2.0 wt%, the content of X is ≤2 wt%, and the balance is Zn. The process for preparing a low-driving-potential Zn-Mn-X alloy sacrificial anode is as follows: First, heat the pure zinc to 550–700°C; Then, add the Zn-Mn master alloy and stir; Finally, the temperature is lowered to 500℃, and one or more of the low-melting-point Ga, Sn, Pb, and Sb are added to the melt. The mixture is stirred and kept at a casting temperature of 430-500℃ for 4-8 minutes to obtain the Zn-Mn-X alloy sacrificial anode. The average grain size of the Zn-Mn-X alloy sacrificial anode is less than 500 μm; the Zn-Mn-X alloy sacrificial anode has an operating potential of -0.75V to -0.94V in seawater and a current efficiency of ≥90%.

2. The low driving potential Zn-Mn-X alloy sacrificial anode according to claim 1, characterized in that, Micron-sized high-potential precipitates formed by low-melting-point alloying elements are distributed at grain boundaries and within grains.

Citation Information

Patent Citations

  • Low-driving potential aluminum alloy sacrificial anode

    CN101445936B

  • A kind of low driving potential aluminum alloy sacrificial anode material and preparation method thereof

    CN105568091B

  • Low-driving-potential aluminum alloy sacrificial anode for seawater and preparation method thereof

    CN110042401A

  • Low driving potential aluminum alloy sacrificial anode for seawater cooling water system and preparation method thereof

    CN115961286B

  • High-temperature zinc alloy sacrificial anode

    CN101705491A