Whitening / perm / repellent one bath fabric processing method

By using a one-bath process for whitening, waterproofing, and wrinkle-free fabrics, the problems of long processing times and high energy consumption in traditional fabric processing are solved. This enables ultra-short processing times and environmentally friendly whitening, wrinkle-free, and waterproof fabric processing while maintaining high performance and environmental friendliness.

CN118147920BActive Publication Date: 2026-11-20LU FENG WEAVING & DYEING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410312978.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2026-11-20
Estimated Expiration
2044-03-19

AI Technical Summary

Technical Problem

Existing whitening, wrinkle-free, and waterproof fabric processing procedures are lengthy, resulting in a lot of wastewater and exhaust gas, high energy consumption, and the use of fluorine-containing additives in traditional waterproofing systems is not environmentally friendly.

Method used

The whitening/waterproofing/iron-free one-bath process is adopted. By mixing whitening agent, iron-freeing agent, waterproofing agent and crosslinking agent under the condition of mutual solubility, combined with bio-based waterproofing agent, whitening, iron-freeing and waterproofing treatment can be completed in one step, reducing the stretching and baking process.

Benefits of technology

Shorten the processing flow, reduce water, electricity and gas consumption, maintain high waterproof performance and wrinkle-free properties, and use bio-based additives that are environmentally friendly and fluorine-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004748109280000071
    Figure BDA0004748109280000071
Patent Text Reader

Abstract

The application belongs to the technical field of textile processing, and particularly relates to a one-bath fabric processing method for whitening / ironing-free / waterproofing. The one-bath fabric processing method for whitening / ironing-free / waterproofing comprises the following steps: pretreating fabric grey cloth, whitening / ironing-free / waterproofing in one bath, and preshrinking, so that an ultra-short-process ironing-free waterproof fabric is obtained. The finishing liquid for whitening / ironing-free / waterproofing in one bath comprises 10-20 g / L of a whitening agent, 80-100 g / L of an ironing-free assistant, 24-30 g / L of a resin catalyst, 150-200 g / L of a waterproofing assistant, 10-15 g / L of a waterproofing crosslinking agent, and the rest of water. The one-bath fabric processing method for whitening / ironing-free / waterproofing provided by the application can shorten the processing steps and reduce energy consumption while ensuring the fabric hand feeling, waterproofing performance, ironing-free property and texture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of textile processing, specifically relating to a one-bath processing method for whitening / iron-free / waterproof fabrics. Background Technology

[0002] The processing of wrinkle-free waterproof fabrics is too long, resulting in a lot of wastewater and exhaust gas. Because of the long process, it also consumes a lot of water, electricity and gas, causing significant environmental pollution and high labor costs.

[0003] The current processing flow for whitening, wrinkle-free, and waterproof fabrics is: whitening -- wrinkle-free -- baking -- waterproofing -- baking -- pre-shrinking. Waste gas is generated during the four processes of wrinkle-free, waterproofing, and baking. Ordinary wrinkle-free waterproof systems require two baking processes, which can easily reduce their whiteness. In ordinary wrinkle-free waterproof systems, the wrinkle-free process is completed on a tenter frame and then dried before baking, and the waterproofing process is completed on a tenter frame and then dried before baking.

[0004] CN114481613A discloses a formaldehyde-free, wrinkle-free, three-proof, and one-bath finishing method for solution-dyed fabrics. The process flow is as follows: fabric preparation, liquid ammonia finishing, application of formaldehyde-free wrinkle-free and three-proof additives, baking, stretching, pre-shrinking, and inspection. The application of formaldehyde-free wrinkle-free and three-proof one-bath additives involves controlling the drying oven temperature at 80-100℃, the fabric surface temperature at 35-40℃, and the fabric humidity at the unloaded point at 6-6.6%. Finally, the fabric is rolled up at the unloaded point. However, the method uses fluorine-containing three-proof additives, which are not environmentally friendly. Drying and baking are performed in separate steps. After high-temperature baking, a baking wash with added additives is required, and acid rolling is necessary on the stretching machine. The process is complex, and the waste gas and wastewater production is significant.

[0005] CN113981685A discloses a processing method for a wrinkle-free and waterproof brushed fabric. The method involves pretreatment of pure cotton or polyester-cotton greige fabric followed by brushing, brushing wash, a one-bath waterproof / wrinkle-free treatment, baking, and pre-shrinking to obtain a wrinkle-free and waterproof brushed fabric. The finishing solution for the one-bath waterproof / wrinkle treatment includes: wrinkle-free resin CR-ZFC, fiber protectant SF-P, and waterproofing agent SA-9. The one-bath waterproof / wrinkle treatment is performed by drying on a tenter frame followed by baking in a baking machine. The resulting brushed fabric is relatively thick and heavy.

[0006] CN116590929A discloses a three-proof fabric, a fabric, and a method for preparing the same, comprising the following steps: cleaning the fabric, removing stains from the fabric, washing and drying, and preparing a three-proof finishing agent; the three-proof finishing agent comprises the following auxiliary components: a fluorine-free waterproofing agent (waterborne polyurethane and polyacrylate polymer or polyurethane polymer), an antistatic agent (hydrophilic silicone oil), a crosslinking agent (waterborne aliphatic isocyanate), and a waterproof penetrating agent BC; padding treatment; applying adhesive tape to the back of the cleaned fabric and padding it, using the three-proof finishing agent as the working solution, padding once and drying, removing the tape, and baking; it is necessary to apply adhesive to the back of the fabric before padding with the three-proof auxiliary agent, and after padding with the three-proof auxiliary agent, it is necessary to dry and then bake; the finished fabric does not have wrinkle-free properties. Summary of the Invention

[0007] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a one-bath whitening / wrinkle-free / waterproof fabric processing method that, while ensuring the fabric's hand feel, waterproof performance, wrinkle-free properties, and texture, shortens the processing steps and reduces energy consumption.

[0008] The fabric processing method of the present invention for whitening / wrinkle-free / waterproof one bath is as follows: the fabric greige is pre-treated → whitening / wrinkle-free / waterproof one bath → pre-shrinking to obtain an ultra-short process wrinkle-free and waterproof fabric.

[0009] The whitening / iron-free / waterproof one-bath finishing solution comprises: whitening agent 10-20g / L, iron-free agent 80-100g / L, resin catalyst 24-30g / L, waterproofing agent 150-200g / L, waterproof crosslinking agent 10-15g / L, and the balance being water.

[0010] The whitening / waterproofing / wrinkle-free one-bath process uses a two-dip, two-roll process with a roll-off rate of 60%-70% and a machine speed of 45-55m / min.

[0011] For whitening / iron-free / waterproofing, a one-bath process is used, which involves pre-drying followed by drying. The pre-drying room temperature is 105-110℃, and the pre-drying time is 40-50 seconds. The drying room temperature is 170-180℃, and the drying time is 30-40 seconds.

[0012] The pretreatment includes singeing, desizing, boiling, bleaching, and mercerizing.

[0013] The wrinkle-free additive is an etherified N-hydroxymethylamine resin, preferably EFR-3.

[0014] The resin catalyst is magnesium chloride, preferably magnesium chloride 531.

[0015] The waterproofing agent is an alkyl urea fluorine-free waterproofing agent, preferably R3.

[0016] The waterproof crosslinking agent is a capped polyisocyanate crosslinking agent, preferably AlN.

[0017] The whitening agent is a derivative of stilbene disulfonic acid, preferably a mixture of EVB, EBB, and BLH.

[0018] Pre-shrinkage speed: 40-60m / min; compression distance: 8-10mm; felt temperature: 80-120℃; rubberized felt temperature: 90-130℃; tension: 2-5kg; adjusting frame tension: 20-50.

[0019] Specifically, the fabric processing method for whitening / wrinkle-free / waterproofing includes the following steps:

[0020] (1) Pretreatment: The fabric is singed, desized, scouring, bleached and mercerized.

[0021] (2) Whitening / Waterproofing / Iron-free one-bath finishing solution: Whitening agent 10-20g / L, iron-freeing agent EFR-3: 80-100g / L, magnesium chloride 531: 24-30g / L, waterproofing agent R3: 150-200g / L, waterproofing crosslinking agent AIN: 10-15g / L, the balance is water; adopt a two-dip two-roll process, with a roll residue rate of 60%-70%, a machine speed of 45-55m / min, pre-drying first, then drying, the pre-drying chamber temperature is 105-110℃, the pre-drying time is 40-50s; the drying chamber temperature is 170-180℃, the drying time is 30-40s.

[0022] (3) Pre-shrinkage: speed: 40-60m / min; pressure distance: 8-10mm; blanket temperature: 80-120℃; rubber blanket temperature: 90-130℃; tension: 2-5kg; adjustment frame tension: 20-50.

[0023] The fabric processing method of the present invention for whitening / wrinkle-free / waterproofing in one bath has an ultra-short process, improving the multi-step method to a one-step method. The whitening / wrinkle-free / waterproofing one bath process reduces two stretching steps and one baking step. Combined with bio-based waterproofing additives, whitening / wrinkle-free / waterproof polyester-cotton fabric is produced.

[0024] This invention uses three types of additives under mutually soluble conditions to act simultaneously on one fabric, achieving whitening, wrinkle-free, and waterproofing in one bath. By adjusting the process parameters of the tenter frame, whitening, wrinkle-free, and waterproofing, which are traditionally accomplished in three steps, can be completed in one step. The fabric is pre-dried in the drying oven at the front end of the tenter frame and then baked in the drying oven at the rear end of the tenter frame, realizing integrated drying and baking.

[0025] Compared with the prior art, the beneficial effects of the present invention are:

[0026] (1) The fabric processing method of the present invention for whitening / iron-free / waterproofing in one bath adopts the whitening / iron-free / iron-free one bath process, which shortens the process flow and reduces the consumption of labor, water and electricity.

[0027] (2) The fabric processing method of the present invention for whitening / iron-free / waterproofing in one bath adopts a mixture of whitening agent, iron-free agent and waterproofing agent, which has good waterproof performance, high iron-free performance, more than 90 points before washing, and more than 80 points after 5 washes.

[0028] (3) The fabric processing method of the present invention for whitening / iron-free / waterproofing uses bio-based waterproofing additives, which is green and environmentally friendly. Detailed Implementation

[0029] The present invention will be further described below with reference to specific embodiments.

[0030] The finishing solutions used in the following examples and comparative examples were all commercially available products:

[0031] The wrinkle-free resin is EFR-3, an etherified N-hydroxymethylamine resin manufactured by Shenzhen Advanced Hualian Fine Chemical Co., Ltd.

[0032] Resin catalyst: Magnesium chloride 531, manufactured by Shenzhen Advanced Hualian Fine Chemical Co., Ltd.

[0033] Waterproofing agent: Alkyl urea fluorine-free waterproofing agent R3, manufactured by Chemours Chemicals (Shanghai) Co., Ltd.; purchased by Shanghai Xinyong Textile Dyeing and Chemical Co., Ltd.

[0034] Waterproof crosslinking agent: End-capped polyisocyanate crosslinking agent AIN, manufactured by Nanjing Chunjing Science and Trade Co., Ltd.

[0035] Brightening agents: Fluorescent brightener EVB, Angco Chemical (China) Co., Ltd.; Fluorescent brightener EBB, Angco Chemical (China) Co., Ltd.

[0036] Fluorescent whitening agent BLH, Angco Chemical (China) Co., Ltd.

[0037] The whitening agents used in the following examples are a mixture of EVB, EBB, and BLH.

[0038] Example 1

[0039] The fabric used in this embodiment is: 23% renewable polyester / 42% ordinary polyester / 35% cotton, T / C45*REPT / C45*135*74*59 / 60 (polyester-cotton 45 count*polyester-cotton 45 count*warp density 135*weft density 74*width 59 / 60 inches), with a 1 / 1 plain weave.

[0040] The aforementioned method for processing whitening / wrinkle-free / waterproof fabric includes the following steps:

[0041] (1) Fabric pretreatment: The greige fabric is successively subjected to singeing, desizing, scouring, bleaching and mercerizing.

[0042] (2) Whitening / Waterproofing / Iron-free one-bath: Mix the finishing liquid according to the following concentrations: whitening agent: 10g / L, iron-free resin EFR-3: 80g / L, resin catalyst 531: 24g / L, waterproofing agent R3: 150g / L, waterproofing crosslinking agent AIN: 10g / L, with the remainder being water; perform two dips and two slits on the treated fabric, with a machine speed of 45m / min and a slit rate of 70%, and set the pre-drying chamber temperature to 110℃ for 40s, and the drying chamber temperature to 170℃ for 40s.

[0043] (3) Pre-shrinkage: vehicle speed 40m / min; pressure distance: 10mm, blanket temperature 100℃, rubber blanket temperature: 100℃, tension: 2kg, adjusting frame tension: 50N.

[0044] Example 2

[0045] The fabric used in this embodiment is: 57.5% cotton / 38.5% polyester / 4% spandex, CVC45*CVC45(SPANDEX40D)*140*80*55 / 56 (polyester-cotton 45 count*polyester-cotton 45 count with spandex 40 denier*warp density 140*weft density 80*width 55 / 56 inches), weave 2 / 1S.

[0046] The aforementioned method for processing whitening / wrinkle-free / waterproof fabric includes the following steps:

[0047] (1) Fabric pretreatment: The greige fabric is successively subjected to singeing, desizing, scouring, bleaching and mercerizing.

[0048] (2) Whitening / Waterproofing / Iron-free one-bath: Mix the finishing liquid according to the following concentrations: whitening agent: 15g / L, iron-free resin EFR-3: 90g / L, resin catalyst 531: 27g / L, waterproofing agent R3: 180g / L, waterproofing crosslinking agent AIN: 12g / L, with the remainder being water; perform two dips and two rolls on the treated fabric, with a machine speed of 55m / min and a roll-off rate of 65%, and set the pre-drying chamber temperature to 105℃ for 45s, and the drying chamber temperature to 175℃ for 35s.

[0049] (3) Pre-shrinkage: speed: 50m / min; pressure distance: 8mm; blanket temperature: 120℃; rubber blanket temperature: 90℃; tension: 3kg; adjustment frame tension: 40N.

[0050] Example 3

[0051] The fabric used in this embodiment is: 35% cotton and 65% polyester, REP T / C45*T / C45*130*80*57 / 58 (45-inch count polyester / cotton*45-inch count polyester / cotton*130 warp density*80 weft density*57 / 58 inches), with a weave of 1 / 1+1 / 3.

[0052] The aforementioned method for processing whitening / wrinkle-free / waterproof fabric includes the following steps:

[0053] (1) Fabric pretreatment: The greige fabric is successively subjected to singeing, desizing, scouring, bleaching and mercerizing.

[0054] (2) Whitening / Waterproofing / Iron-free one-bath: Mix the finishing liquid according to the following concentrations: whitening agent: 20g / L, iron-free resin EFR-3: 100g / L, resin catalyst 531: 30g / L, waterproofing agent R3: 200g / L, waterproofing crosslinking agent AIN: 15g / L, with the remainder being water; perform two dips and two rolls on the treated fabric, with a machine speed of 50m / min and a roll-off rate of 60%, a pre-drying chamber temperature of 105℃ for 50s, and a drying chamber temperature of 180℃ for 30s.

[0055] (3) Pre-shrinkage: speed: 60m / min; pressure distance: 9mm; blanket temperature: 80℃; rubber blanket temperature: 130℃; tension: 5kg; adjustment frame tension: 20N.

[0056] Comparative Example 1

[0057] The fabric used in this comparative example is: 23% renewable polyester / 42% regular polyester / 35% cotton, T / C45*REPT / C45*135*74*59 / 60 (polyester-cotton 45 count*polyester-cotton 45 count*warp density 135*weft density 74*width 59 / 60 inches), 1 / 1 plain weave.

[0058] The aforementioned method for processing whitening, wrinkle-free, and waterproof fabrics includes the following steps:

[0059] (1) Fabric pretreatment: The greige fabric is successively subjected to singeing, desizing, scouring, bleaching and mercerizing.

[0060] (2) Whitening: Whitening agent: 10g / L, the remainder is water, the roll residue rate is 70%, two dips and two rolls, machine speed 45m / min, the drying room temperature is set to 170℃ for drying time 40S.

[0061] (3) No ironing: No ironing resin EFR-3: 80g / L, resin catalyst 531: 24g / L, the balance is water, two dips and two rolls, machine speed 45m / min, roll residue rate 70%, drying room temperature set to 130℃ for 40S.

[0062] (4) Baking: speed 50m / min, oven temperature 150℃, time 150s.

[0063] (5) Waterproofing: Waterproofing agent R3: 150g / L, waterproofing crosslinking agent AIN: 10g / L, the remainder is water, two dips and two rolls, machine speed 45m / min, roll residue rate 70%, drying room temperature set to 130℃ for 40S.

[0064] (6) Baking: speed 50m / min, oven temperature 150℃, time 150s.

[0065] (7) Pre-shrinkage: machine speed 40m / min; compression distance: 10mm, felt temperature 100℃, rubberized felt temperature: 100℃. Comparative Example 2

[0066] The fabric used in this comparative example is: 57.5% cotton / 38.5% polyester / 4% spandex, CVC45*CVC45(SPANDEX40D)*140*80*55 / 56 (45-count polyester / cotton*45-count polyester / cotton with 40 denier spandex*140 warp density*80 weft density*55 / 56 inches), 2 / 1S weave.

[0067] The aforementioned method for processing whitening, wrinkle-free, and waterproof fabrics includes the following steps:

[0068] (1) Fabric pretreatment: The greige fabric is successively subjected to singeing, desizing, scouring, bleaching and mercerizing.

[0069] (2) Whitening: Whitening agent: 15g / L, the remainder is water, two dips and two rolls, the roll residue rate is 65%, machine speed: 55m / min, drying room temperature 175℃, time 35S.

[0070] (3) No ironing: No ironing resin EFR-3: 90g / L, resin catalyst 531: 27g / L, the balance is water, two dips and two rolls, the roll residue rate is 65%, the machine speed is 55m / min, the oven temperature is 135℃, and the time is 35S.

[0071] (4) Baking: speed 50m / min, oven temperature 150℃, time 150s.

[0072] (5) Waterproofing: Waterproofing agent R3: 180g / L, waterproofing crosslinking agent AIN: 12g / L, the remainder is water, two dips and two rolls, roll residue rate is 65%, machine speed: 55m / min, drying room temperature 135℃, time 35S.

[0073] (6) Baking: speed 50m / min, oven temperature 150℃, time 150s.

[0074] (7) Pre-shrinkage: speed: 50m / min; pressure distance: 8mm; blanket temperature: 120℃; rubber blanket temperature: 90℃; tension: 3kg; adjusting frame tension: 40N.

[0075] Comparative Example 3

[0076] The fabric used in this comparative example is 35% cotton and 65% polyester, REP T / C45*T / C45*130*80*57 / 58 (45 English count polyester / cotton*45 English count polyester / cotton*warp density 130*weft density 80*width 57 / 58 inches), with a weave of 1 / 1+1 / 3.

[0077] The aforementioned method for processing whitening, wrinkle-free, and waterproof fabrics includes the following steps:

[0078] (1) Fabric pretreatment: The greige fabric is successively subjected to singeing, desizing, scouring, bleaching and mercerizing.

[0079] (2) Whitening: Whitening agent: 20g / L, balance is water, two dips and two rolls, roll residue rate is 60%, machine speed: 50m / min, drying oven temperature: 180℃, time: 30s

[0080] (3) Wrinkle-free: Wrinkle-free resin EFR-3: 100g / L, resin catalyst 531: 30g / L, balance is water, two dips and two rolls, roll residue rate is 60%, machine speed: 50m / min, drying oven temperature 130℃, time 30s

[0081] (4) Baking: speed 50m / min, oven temperature 150℃, time 150s.

[0082] (5) Waterproofing: Waterproofing agent R3: 200g / L, waterproofing crosslinking agent AIN: 15g / L, the remainder is water, two dips and two rolls, roll residue rate is 60%, machine speed: 50m / min, drying room temperature 130℃, time 30S.

[0083] (6) Baking: speed 50m / min, oven temperature 150℃, time 150s.

[0084] (3) Pre-shrinkage: speed: 60m / min; pressure distance: 9mm; blanket temperature: 80℃; rubber blanket temperature: 130℃; tension: 5kg; adjustment frame tension: 20N.

[0085] The wrinkle-free waterproof fabrics prepared in the above examples and comparative examples were subjected to performance testing. The test results and test standards are shown in Table 1.

[0086] Table 1 Test Results and Test Standards

[0087]

[0088] As can be seen from the table above, the processing method of the ultra-short process wrinkle-free waterproof fabric of the present invention reduces the decrease in whiteness. While maintaining the waterproof effect and wrinkle-free properties, it reduces power consumption by 0.5 kWh per meter of fabric and reduces water consumption by 4 liters. The bio-based waterproofing additives used are fluorine-free and environmentally friendly.

[0089] Of course, the above description is only a preferred embodiment of the present invention and should not be considered as limiting the scope of the embodiments of the present invention. The present invention is also not limited to the above examples, and all equivalent changes and improvements made by those skilled in the art within the scope of the present invention should fall within the patent coverage of the present invention.

Claims

1. A method for processing a whitening / wrinkle-free / waterproof fabric in one bath, characterized in that: The fabric is pre-treated → whitening / iron-free / waterproofing in one bath → pre-shrinking to obtain an ultra-short process iron-free and waterproof fabric; the whitening, iron-freeing and waterproofing are completed in one step, the fabric is pre-dried in the front oven of the tenter frame, and then baked in the rear oven of the tenter frame to achieve integrated drying and baking. The whitening / iron-free / waterproof one-bath finishing solution comprises: whitening agent 10-20g / L, iron-free agent: 80-100g / L, resin catalyst: 24-30g / L, waterproofing agent: 150-200g / L, waterproof crosslinking agent: 10-15g / L, and the balance is water. For whitening / iron-free / waterproofing, a one-bath process is used, which involves pre-drying followed by baking. The pre-drying temperature is 105-110℃ and the pre-drying time is 40-50 seconds. The baking temperature is 170-180℃ and the baking time is 30-40 seconds. The waterproof crosslinking agent is a capped polyisocyanate crosslinking agent; the wrinkle-free additive is an etherified N-hydroxymethylamine resin; the resin catalyst is magnesium chloride; and the waterproof additive is an alkyl urea fluorine-free waterproof additive.

2. The fabric processing method for whitening / wrinkle-free / waterproof fabric according to claim 1, characterized in that: The whitening / waterproofing / wrinkle-free one-bath process uses a two-dip, two-roll process with a roll-off rate of 60%-70% and a machine speed of 45-55m / min.

3. The fabric processing method for whitening / wrinkle-free / waterproof fabric according to claim 1, characterized in that: The pretreatment processes include singeing, desizing, boiling, bleaching, and mercerizing.

4. The fabric processing method for whitening / wrinkle-free / waterproof fabric according to claim 1, characterized in that: Pre-shrinkage speed: 40-60m / min; compression distance: 8-10mm; felt temperature: 80-120℃; rubberized felt temperature: 90-130℃; tension: 2-5kg; adjusting frame tension: 20-50.

Citation Information

Patent Citations

  • Processing method of non-ironing and waterproof sanded fabric

    CN113981685A