A multi-metal oxide and a method for preparing the same and a wastewater treatment application

A simple one-step method for preparing CuO/ZnFe₂O₄ catalyst has solved the problem of low removal efficiency of organic pollutants in high-salt wastewater, achieving efficient and stable advanced oxidation water treatment effect, and is suitable for the treatment of high-salt organic wastewater.

CN118162143BActive Publication Date: 2026-11-24UNIV OF SCI & TECH OF CHINA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410275427.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-11
Publication Date
2026-11-24
Estimated Expiration
2044-03-11

AI Technical Summary

Technical Problem

Existing advanced oxidation water treatment technologies based on persulfate are not very effective in treating high-salt wastewater, mainly because reactive oxygen species are quenched by high-concentration inorganic salt ions, resulting in low removal efficiency of target organic pollutants. There is also a lack of large-scale and efficient advanced oxidation catalysts.

Method used

A simple one-step method was used to prepare a composite catalyst of CuO and spinel-type oxide ZnFe₂O₄. CuO nanoparticles were prepared by sol-gel method and supported on the surface of sheet-like ZnFe₂O₄ to serve as a persulfate catalyst for the non-radical oxidation of organic pollutants.

Benefits of technology

It achieves efficient activation of persulfate oxidation of organic pollutants in high-salt environments, exhibiting superior salt tolerance, good catalytic activity and stability, and is suitable for the efficient and low-consumption treatment of high-salt organic wastewater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118162143B_ABST
    Figure CN118162143B_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing polymetallic oxides, comprising the following steps: A) mixing a mixed metal salt solution containing zinc, iron, and copper salts with a chelating agent to perform a sol-gel reaction to obtain a precursor; B) drying and calcining the precursor to obtain a CuO / ZnFe2O4 catalyst. This invention prepares polymetallic oxides, represented by CuO nanoparticle-supported sheet-like ZnFe2O4 spinel catalysts (CuO / ZnFe2O4), via a sol-gel method. The preparation method is simple, economical, and can be applied on a large scale. By introducing a non-radical oxidation pathway through CuO, efficient activation of persulfate oxidation of organic pollutants is achieved in high-salt environments. The prepared material exhibits superior salt tolerance, good catalytic activity, and stability, and can be used as a catalyst to activate persulfate, achieving efficient and low-consumption treatment of high-salt organic wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of advanced oxidation water treatment technology, specifically relating to a multi-metal oxide, its preparation method, and its application in wastewater treatment. Background Technology

[0002] Persulfate-based advanced oxidation technologies (PS-AOPs) have shown great potential in treating organic wastewater, but their effectiveness is poor when applied to high-salinity wastewater. The main reason is that reactive oxygen species such as sulfate radicals and hydroxyl radicals generated in the PS-AOPs system are easily quenched or transformed by high concentrations of inorganic salt ions, leading to a significant reduction in the removal efficiency of the target organic pollutants. Developing non-radical-based advanced oxidation systems is one of the important strategies to solve this problem, with optimized catalyst design being crucial.

[0003] Transition metal oxides can serve as catalysts for activating persulfates, possessing advantages such as abundant elemental reserves, high catalytic efficiency, and ease of mass production. Spinel-type oxides, in particular, exhibit stable structures and are easily modulated to form various composite materials, making them ideal catalysts for developing non-radical advanced oxidation systems. However, the salt tolerance of these catalysts remains limited, and their preparation process (generally employing a two-step synthesis method) is complex, hindering large-scale production and application. In summary, a high-performance advanced oxidation catalyst that can be prepared on a large scale and applied to high-salt organic wastewater is still lacking. Summary of the Invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide a polymetallic oxide and its preparation method and its application in wastewater treatment. The present invention uses a simple one-step method to prepare a composite catalyst of CuO and spinel-type oxide ZnFe2O4, which enhances the decontamination effect of the system and improves the salt resistance, and has broad application prospects in the control of advanced oxidation water pollution in complex water bodies.

[0005] This invention provides a method for preparing a polymetallic oxide, comprising the following steps:

[0006] A) A mixed metal salt solution containing zinc, iron, and copper salts is mixed with a chelating agent and subjected to a sol-gel reaction to obtain a precursor;

[0007] B) The precursor is dried and calcined to obtain CuO / ZnFe2O4 catalyst.

[0008] Preferably, the zinc salt is one of zinc acetate, zinc nitrate, zinc sulfate, zinc carbonate, and zinc chloride;

[0009] The iron salt is one of the following: iron acetate, iron nitrate, iron sulfate, iron carbonate, and iron chloride;

[0010] The copper salt is one of copper acetate, copper nitrate, copper sulfate, copper carbonate, and copper chloride;

[0011] The molar ratio of the zinc salt, iron salt, and copper salt is (0.5–2.0):(0.5–2.0):(0.5–2.0).

[0012] Preferably, the sol-gel reaction includes the following steps:

[0013] A mixed metal salt solution containing zinc, iron, and copper salts was heated and stirred in a water bath, during which a chelating agent was added and the temperature was increased.

[0014] Preferably, the chelating agent is selected from at least one of citric acid, glycine, oxalic acid, ethylenediaminetetraacetic acid (EDTA), and polyvinylpyrrolidone (PVP);

[0015] The molar amount of the chelating agent used is the sum of the amounts of zinc salt, iron salt, and copper salt.

[0016] The water bath heating temperature is 60℃~90℃, and the time is 5h~6h;

[0017] The chelating agent is added after heating in a 60°C water bath and stirring for 1 hour.

[0018] The heating process takes place 2 hours after adding the chelating agent and stirring thoroughly.

[0019] Preferably, the drying temperature is 60-90°C and the drying time is 18-24 hours;

[0020] The calcination conditions are as follows: the precursor is heated from room temperature to 400℃ to 500℃ at a rate of 3 to 6℃ / min and held for 2 to 4 hours, followed by natural cooling.

[0021] The present invention also provides a CuO / ZnFe2O4 catalyst, wherein the catalyst is CuO nanoparticles supported on the surface of a sheet-like spinel metal oxide ZnFe2O4.

[0022] The present invention also provides an application of the above-mentioned CuO / ZnFe2O4 catalyst in the removal of organic pollutants from water.

[0023] This invention also provides a method for treating high-salt, recalcitrant organic wastewater, comprising the following steps:

[0024] An oxidant and the catalyst are added to a high-salinity water body containing organic pollutants to carry out a reaction.

[0025] Preferably, the dosage of the catalyst is 0.05 g / L to 0.20 g / L;

[0026] The oxidant is one of persulfate (PDS), permonsulfate (PMS), hydrogen peroxide (H2O2), or periodate (PI), and the dosage is 0.2 mM to 2.0 mM.

[0027] Preferably, the organic pollutants include, but are not limited to, tetracycline (TC), acetaminophen (PCM), bisphenol A (BPA), and 4-chlorophenol (4-CP), with a concentration of 5.0–20.0 mg / L;

[0028] The salt ions in the high-salt water body include, but are not limited to, chloride ions (Cl). - ), dihydrogen phosphate ions (H2PO4) - ), bicarbonate ions (HCO3) - ) and nitrate ions (NO3) - One or more of the following, with a concentration of 100mM to 1000mM.

[0029] Compared with existing technologies, this invention provides a method for preparing polymetallic oxides, comprising the following steps: A) mixing a mixed metal salt solution containing zinc, iron, and copper salts with a chelating agent to perform a sol-gel reaction to obtain a precursor; B) drying and calcining the precursor to obtain a CuO / ZnFe2O4 catalyst. This invention prepares polymetallic oxides, represented by CuO nanoparticle-supported sheet-like ZnFe2O4 spinel catalysts (CuO / ZnFe2O4), via a sol-gel method. The preparation method is simple, economical, and can be applied on a large scale. By introducing a non-radical oxidation pathway through CuO, efficient activation of persulfate oxidation of organic pollutants is achieved in high-salt environments. The obtained material exhibits superior salt tolerance, good catalytic activity, and stability, and can be used as a catalyst to activate persulfate, achieving efficient and low-consumption treatment of high-salt organic wastewater. Attached Figure Description

[0030] Figure 1 A schematic diagram of the synthesis route of the polymetallic oxide catalyst provided by the present invention;

[0031] Figure 2 The XRD patterns of the CuO / ZnFe2O4 catalyst obtained in Example 1 and the ZnFe2O4 catalyst obtained in Comparative Example 1 are shown below.

[0032] Figure 3 SEM characterization images of the CuO / ZnFe2O4 catalyst obtained in Example 1 and the ZnFe2O4 catalyst obtained in Comparative Example 1;

[0033] Figure 4 A performance comparison chart of different reaction systems constructed from the PDS system alone, the CuO / ZnFe2O4 catalyst obtained in Example 1, and the ZnFe2O4 catalyst obtained in Comparative Example 1;

[0034] Figure 5 The graph shows the TC removal performance of the CuO / ZnFe2O4 catalyst obtained in Example 1 and the PDS oxidation system under different pH conditions.

[0035] Figure 6 A comparison diagram of the TC oxidation mechanism of CuO / ZnFe2O4 catalyst obtained in Example 1 and ZnFe2O4 catalyst obtained in Comparative Example 1 with the PDS system;

[0036] Figure 7 The diagram shows the salt tolerance of the CuO / ZnFe2O4 catalyst obtained in Example 1.

[0037] Figure 8 The graph shows the chlorine resistance of the CuO / ZnFe2O4 catalyst obtained in Example 1.

[0038] Figure 9 The stability diagram of the CuO / ZnFe2O4 catalyst obtained in Example 1 is shown. Detailed Implementation

[0039] This invention provides a method for preparing a polymetallic oxide, comprising the following steps:

[0040] A) A mixed metal salt solution containing zinc, iron, and copper salts is mixed with a chelating agent and subjected to a sol-gel reaction to obtain a precursor;

[0041] B) The precursor is dried and calcined to obtain CuO / ZnFe2O4 catalyst.

[0042] The present invention first prepares a mixed metal salt solution containing zinc salt, iron salt and copper salt.

[0043] Specifically, the zinc salt, iron salt, and copper salt are dispersed in a solvent and mixed evenly to obtain a mixed metal salt solution containing zinc salt, iron salt, and copper salt.

[0044] The zinc salt is one of zinc acetate, zinc nitrate, zinc sulfate, zinc carbonate, and zinc chloride;

[0045] The iron salt is one of the following: iron acetate, iron nitrate, iron sulfate, iron carbonate, and iron chloride;

[0046] The copper salt is one of copper acetate, copper nitrate, copper sulfate, copper carbonate, and copper chloride;

[0047] The molar ratio of the zinc salt, iron salt, and copper salt is (0.5–2.0):(0.5–2.0):(0.5–2.0), preferably 1:1:1, 0.5:1:1.5, 0.5:1.5:1, or any value between (0.5–2.0):(0.5–2.0):(0.5–2.0).

[0048] The solvent includes at least one of deionized water, ethanol, acetone, and ethylene glycol.

[0049] Next, the mixed metal salt solution is mixed with a chelating agent to carry out a sol-gel reaction, which includes the following steps:

[0050] A mixed metal salt solution containing zinc, iron, and copper salts was heated and stirred in a water bath, during which a chelating agent was added and the temperature was increased.

[0051] The chelating agent is selected from at least one of citric acid, glycine, oxalic acid, ethylenediaminetetraacetic acid (EDTA), and polyvinylpyrrolidone (PVP).

[0052] The molar amount of the chelating agent used is the sum of the amounts of zinc salt, iron salt, and copper salt.

[0053] The water bath heating temperature is 60℃~90℃, and can be any value between 60℃, 70℃, 80℃, 90℃, or 60℃~90℃, and the time is 5h~6h;

[0054] The chelating agent is added after heating in a 60°C water bath and stirring for 1 hour.

[0055] The heating process takes place 2 hours after adding the chelating agent and stirring thoroughly.

[0056] The stirring is intended to ensure that the solutes are mixed evenly to form a homogeneous sol and gel. Conventional stirring speeds in the art can achieve this effect, therefore no limitation is placed on the stirring speed.

[0057] Finally, the precursor was dried and calcined to obtain the CuO / ZnFe2O4 catalyst.

[0058] The drying temperature is 60-90℃, preferably 60, 70, 80, 90℃, or any value between 60-90℃, and the drying time is 18h-24h.

[0059] The calcination conditions are as follows: the precursor is heated from room temperature to 400℃ to 500℃ at a rate of 3 to 6℃ / min and held for 2 to 4 hours, followed by natural cooling.

[0060] The preferred heating rate for calcination is 3, 4, 5, or 6, or any value between 3 and 6 °C / min. The preferred calcination temperature is 400, 420, 440, 450, 460, 470, 480, or 500 °C, or any value between 400 °C and 500 °C. The preferred calcination time is 2, 3, or 4 hours, or any value between 2 and 4 hours.

[0061] See Figure 1 , Figure 1 This is a schematic diagram of the synthesis route for the polymetallic oxide catalyst provided by the present invention.

[0062] The present invention also provides a CuO / ZnFe2O4 catalyst prepared by the above preparation method, wherein the catalyst is CuO nanoparticles supported on the surface of a sheet-like spinel metal oxide ZnFe2O4, wherein the average diameter of the CuO nanoparticles is 2±0.2 nm.

[0063] The present invention also provides an application of the above-mentioned CuO / ZnFe2O4 catalyst in the removal of organic pollutants from water.

[0064] This invention also provides a method for treating high-salt, recalcitrant organic wastewater, comprising the following steps:

[0065] An oxidant and the catalyst mentioned above are added to a high-salinity water body containing organic pollutants to carry out a reaction, thereby oxidizing and removing the organic pollutants from the water body and achieving water purification.

[0066] The dosage of the catalyst is 0.05 g / L to 0.20 g / L, and can be any value between 0.05, 0.06, 0.08, 0.10, 0.11, 0.13, 0.15, 0.16, 0.18, 0.20, or 0.05 g / L to 0.20 g / L.

[0067] The oxidant is one of persulfate (PDS), permonsulfate (PMS), hydrogen peroxide (H2O2), and periodate (PI), and the dosage is 0.2 mM to 2.0 mM, which can be any value between 0.2, 0.4, 0.5, 0.6, 0.8, 1.0, 1.2, 1.4, 1.5, 1.6, 1.8, 2.0, or 0.2 mM to 2.0 mM.

[0068] The organic pollutants include, but are not limited to, tetracycline (TC), acetaminophen (PCM), bisphenol A (BPA), and 4-chlorophenol (4-CP), with a concentration of 5.0 to 20.0 mg / L, which can be any value between 5, 10, 15, 20, or 5.0 to 20.0 mg / L.

[0069] The salt ions in the high-salt water body include, but are not limited to, chloride ions (Cl).- ), dihydrogen phosphate ions (H2PO4) - ), bicarbonate ions (HCO3) - ) and nitrate ions (NO3) - One or more of the following, with a concentration of 100mM to 1000mM, which can be 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, or any value between 100mM and 1000mM.

[0070] During the reaction, stirring is performed simultaneously to ensure sufficient contact between the catalyst and persulfate, thereby facilitating the generation of active species and efficient removal of pollutants. Conventional stirring speeds in the art are sufficient to achieve this effect; therefore, no limitation is placed on the stirring speed.

[0071] Unless otherwise specified, all measurements in this invention are performed at room temperature.

[0072] Compared with existing advanced oxidation wastewater treatment technologies, the advanced oxidation wastewater treatment technology using CuO / ZnFe2O4 catalyst provided by this invention has the following superior effects:

[0073] (1) The CuO / ZnFe2O4 catalyst preparation method provided by the present invention is simple in process and easy to operate, and can be applied and expanded on a large scale.

[0074] (2) The present invention selects CuO / ZnFe2O4 catalyst as activator of persulfate. Its structure is CuO nanoparticles supported on sheet-like ZnFe2O4, which can improve its catalytic activity and salt tolerance while maintaining the environmentally friendly and economic advantages of ZnFe2O4.

[0075] (3) The CuO / ZnFe2O4 catalyst provided by the present invention is highly efficient, stable and low toxic. Compared with CuO alone as a catalyst, it can achieve efficient activation of persulfate in a wider pH range. It can still maintain high catalytic activity after multiple cycles of use, and Cu ions are leached out less during the reaction process.

[0076] (4) The CuO / ZnFe2O4 / PDS high-efficiency catalytic oxidation system constructed in this invention can simultaneously generate highly active free radicals and non-free radical active species, and oxidize organic pollutants through multiple pathways to achieve water purification.

[0077] (5) The CuO / ZnFe2O4 / PDS high-efficiency catalytic oxidation system constructed in this invention has high salt tolerance and is suitable for various high-salt organic wastewaters.

[0078] To further understand the present invention, the following embodiments illustrate the polymetallic oxides and their preparation methods, as well as their applications in wastewater treatment. The scope of protection of the present invention is not limited to the following embodiments. Unless otherwise stated, the raw materials and reagents used in the embodiments of the present invention are conventionally available commercially available raw materials and reagents.

[0079] Example 1

[0080] A CuO / ZnFe2O4 catalyst, prepared by the following method: Figure 1 As shown, the specific operation steps are as follows:

[0081] S1. Dissolve 1.1900g (4mM)Zn(NO3)2·6H2O, 1.6160g (4mM)Fe(NO3)3·9H2O, and 0.9664g (4mM)Cu(NO3)3·3H2O in 50mL of water and stir thoroughly to obtain a mixed solution.

[0082] S2. The mixed solution described in S1 is heated in a water bath at 60°C and stirred for 1 hour. Then, 2.5217 g (12 mM) CA is added, and the mixture is heated in a water bath and stirred for another 2 hours. Then, the temperature is raised to 90°C and heated for 4 hours to form a gel, thus obtaining the precursor.

[0083] S3. The precursor described in S2 is dried at 80°C for 24 hours, then calcined at 400°C for 3 hours, and ground to obtain CuO / ZnFe2O4 catalyst.

[0084] Example 2

[0085] A CuO / ZnFe2O4 catalyst is prepared by the following steps:

[0086] S1. Dissolve 0.5950g (2mM) Zn(NO3)2·6H2O, 1.6160g (4mM) Fe(NO3)3·9H2O, and 1.4496g (6mM) Cu(NO3)3·3H2O in 50mL of water and stir thoroughly to obtain a mixed solution.

[0087] S2. The mixed solution described in S1 is heated in a water bath at 60°C and stirred for 1 hour. Then, 2.5217 g (12 mM) CA is added, and the mixture is heated in a water bath and stirred for another 2 hours. Then, the temperature is raised to 90°C and heated for 4 hours to form a gel, thus obtaining the precursor.

[0088] S3. The precursor described in S2 is dried at 80°C for 24 hours, then calcined at 400°C for 3 hours, and ground to obtain CuO / ZnFe2O4 catalyst.

[0089] Example 3

[0090] A CuO / ZnFe2O4 catalyst is prepared by the following steps:

[0091] S1. Dissolve 0.5950g (2mM) Zn(NO3)2·6H2O, 2.4240g (6mM) Fe(NO3)3·9H2O, and 0.9664g (4mM) Cu(NO3)3·3H2O in 50mL of water and stir thoroughly to obtain a mixed solution.

[0092] S2. The mixed solution described in S1 is heated in a water bath at 60°C and stirred for 1 hour. Then, 2.5217 g (12 mM) CA is added, and the mixture is heated in a water bath and stirred for another 2 hours. Then, the temperature is raised to 90°C and heated for 4 hours to form a gel, thus obtaining the precursor.

[0093] S3. The precursor described in S2 is dried at 80°C for 24 hours, then calcined at 400°C for 3 hours, and ground to obtain CuO / ZnFe2O4 catalyst.

[0094] Example 4

[0095] A CuO / ZnFe2O4 catalyst is prepared by the following steps:

[0096] S1. Dissolve 1.1900g (4mM)Zn(NO3)2·6H2O, 1.6160g (4mM)Fe(NO3)3·9H2O, and 0.9664g (4mM)Cu(NO3)3·3H2O in 50mL of water and stir thoroughly to obtain a mixed solution.

[0097] S2. The mixed solution described in S1 is heated in a water bath at 60°C and stirred for 1 hour. Then, 2.5217 g (12 mM) CA is added, and the mixture is heated in a water bath and stirred for another 2 hours. Then, the temperature is raised to 90°C and heated for 4 hours to form a gel, thus obtaining the precursor.

[0098] S3. The precursor described in S2 is dried at 80°C for 24 hours, calcined at 450°C for 3 hours, and then ground to obtain CuO / ZnFe2O4 catalyst.

[0099] Example 5

[0100] A CuO / ZnFe2O4 catalyst is prepared by the following steps:

[0101] S1. Dissolve 1.1900g (4mM)Zn(NO3)2·6H2O, 1.6160g (4mM)Fe(NO3)3·9H2O, and 0.9664g (4mM)Cu(NO3)3·3H2O in 50mL of water and stir thoroughly to obtain a mixed solution.

[0102] S2. The mixed solution described in S1 is heated in a water bath at 60°C and stirred for 1 hour. Then, 2.5217 g (12 mM) CA is added, and the mixture is heated in a water bath and stirred for another 2 hours. Then, the temperature is raised to 90°C and heated for 4 hours to form a gel, thus obtaining the precursor.

[0103] S3. The precursor described in S2 is dried at 80°C for 24 hours, calcined at 500°C for 3 hours, and then ground to obtain CuO / ZnFe2O4 catalyst.

[0104] Comparative Example 1

[0105] A ZnFe2O4 catalyst is prepared by the following steps:

[0106] S1. Dissolve 1.18996g (4mM) Zn(NO3)2·6H2O and 3.232g (8mM) Fe(NO3)3·9H2O in 50mL of water and stir thoroughly to obtain a mixed solution;

[0107] S2. The mixed solution described in S1 is heated in a water bath at 60°C and stirred for 1 hour. Then, 2.5217 g (12 mM) CA is added, and the mixture is heated in a water bath and stirred for another 2 hours. Then, the temperature is raised to 90°C and heated for 4 hours to form a gel, thus obtaining the precursor.

[0108] S3. The precursor described in S2 is dried at 80°C for 24 hours, calcined at 400°C for 3 hours, and then ground to obtain the ZnFe2O4 catalyst.

[0109] Comparative Example 2

[0110] A zinc-copper oxide catalyst is prepared by the following steps:

[0111] S1. Dissolve 1.7850g (6mM) Zn(NO3)2·6H2O and 1.4496g (6mM) Cu(NO3)3·3H2O in 50mL of water and stir thoroughly to obtain a mixed solution;

[0112] S2. The mixed solution described in S1 is heated in a water bath at 60°C and stirred for 1 hour. Then, 2.5217 g (12 mM) CA is added, and the mixture is heated in a water bath and stirred for another 2 hours. Then, the temperature is raised to 90°C and heated for 4 hours to form a gel, thus obtaining the precursor.

[0113] S3. The precursor described in S2 is dried at 80°C for 24 hours, then calcined at 400°C for 3 hours, and ground to obtain a zinc-copper oxide catalyst.

[0114] Comparative Example 3

[0115] An iron-copper oxide catalyst is prepared by the following steps:

[0116] S1. Dissolve 2.4240g (6mM)Fe(NO3)3·9H2O and 1.4496g (6mM)Cu(NO3)3·3H2O in 50mL of water and stir thoroughly to obtain a mixed solution;

[0117] S2. The mixed solution described in S1 is heated in a water bath at 60°C and stirred for 1 hour. Then, 2.5217 g (12 mM) CA is added, and the mixture is heated in a water bath and stirred for another 2 hours. Then, the temperature is raised to 90°C and heated for 4 hours to form a gel, thus obtaining the precursor.

[0118] S3. The precursor described in S2 is dried at 80°C for 24 hours, then calcined at 400°C for 3 hours, and ground to obtain an iron-copper oxide catalyst.

[0119] Example 6

[0120] Polymetallic oxide catalysts for the removal of total chloride (TC) from water

[0121] Take 5.0 mg of the multi-metal oxide catalysts obtained in Examples 1-5 and Comparative Examples 1-3, and add them to 50 mL of TC solution (10 mg / L) with 2.0 mM PDS respectively to start the reaction. During the reaction, at certain time intervals (0, 2 min, 5 min, 10 min, 15 min, 20 min, 30 min, 45 min, 60 min), take 1 mL of the reaction solution, filter it, and add it to 80 μL of 0.25 g / L Na2S2O3 solution to terminate the reaction. The absorbance is measured at a wavelength of 357 nm using a UV spectrophotometer, and the TC removal rate is calculated.

[0122] To provide a control, the performance of TC removal was evaluated using catalyst adsorption alone and PDS oxidation alone.

[0123] Polymetallic oxide catalysts for the adsorption and removal of TC:

[0124] Take 5.0 mg of the multi-metal oxide catalysts obtained in Examples 1-5 and Comparative Examples 1-3, and add them to 50 mL of TC solution (10 mg / L) respectively to start the reaction. During the reaction, take 1 mL of the reaction solution at certain time intervals, filter it, and use a UV spectrophotometer to measure the absorbance at a wavelength of 357 nm to calculate the TC removal rate.

[0125] PDS oxidant alone removes TC through oxidation:

[0126] Add 2.0 mM PDS to 50 mL of TC solution (10 mg / L) to start the reaction. During the reaction, at certain time intervals, take 1 mL of the reaction solution, filter it, and add it to 80 μL of 0.25 g / L Na2S2O3 solution to terminate the reaction. Use a UV spectrophotometer to measure the absorbance at a wavelength of 357 nm and calculate the TC removal rate.

[0127] Example 7

[0128] CuO / ZnFe2O4 is used for the removal of total chloride (TC) from different high-salinity waters.

[0129] Different sodium salts (sodium chloride, sodium dihydrogen phosphate, sodium bicarbonate, and sodium nitrate) were added to 50 mL of TC solution (10 mg / L) at 500 mM each to obtain a high-salt TC solution. 5.0 mg of the CuO / ZnFe2O4 catalyst obtained in Example 1 and 2.0 mM PDS were added to the above high-salt TC solution to initiate the reaction. During the reaction, at certain time intervals, 1 mL of the reaction solution was filtered and added to 80 μL of 0.25 g / L Na2S2O3 solution to terminate the reaction. The absorbance was measured at 357 nm using a UV spectrophotometer, and the TC removal rate was calculated.

[0130] Example 8

[0131] Operational stability of CuO / ZnFe2O4 for removing total chloride (TC) from water

[0132] 5.0 mg of the CuO / ZnFe2O4 catalyst obtained in Example 1 and 2.0 mM PDS were added to 50 mL of TC solution (10 mg / L) to initiate the reaction. During the reaction, at certain time intervals, 1 mL of the reaction solution was filtered and added to 80 μL of 0.25 g / L Na2S2O3 solution to terminate the reaction. The absorbance was measured at 357 nm using a UV spectrophotometer, and the TC removal rate was calculated. After the reaction, the catalyst material was collected by filtration and washed several times with deionized water. The above steps were repeated for a total of 5 cycles, with each cycle lasting 60 min.

[0133] Material property analysis

[0134] (1) X-ray diffraction (XRD) test

[0135] XRD phase analysis was performed on the CuO / ZnFe2O4 catalyst synthesized in Example 1 and the ZnFe2O4 catalyst synthesized in Comparative Example 1. The results are as follows: Figure 2 As shown.

[0136] The results show that the XRD patterns of both CuO / ZnFe2O4 prepared in Example 1 and ZnFe2O4 prepared in Comparative Example 1 correspond well with the standard PDF card of ZnFe2O4. The characteristic peaks of CuO / ZnFe2O4 material also match the standard characteristic peaks of CuO, further demonstrating that the preparation method is successful and effective.

[0137] (2) Scanning electron microscopy (SEM) test

[0138] The CuO / ZnFe2O4 catalyst synthesized in Example 1 and the ZnFe2O4 catalyst synthesized in Comparative Example 1 were analyzed by SEM, and the results are as follows: Figure 3 As shown.

[0139] The results showed that the ZnFe2O4 catalyst had a distinct plate-like structure, and the CuO nanoparticles in the CuO / ZnFe2O4 catalyst were supported on the plate-like ZnFe2O4, with an average diameter of 2±0.2 nm.

[0140] (3) Analysis of catalytic oxidation performance and mechanism

[0141] The removal efficiency of polymetallic oxides from Examples 1-5 and Comparative Examples 1-3 on TC was tested as adsorbent and catalyst, respectively (see Example 6 for specific methods). The results are shown in Table 1.

[0142] Table 1. Test results of catalyst oxidation and adsorption performance

[0143]

[0144]

[0145] The CuO / ZnFe2O4 catalyst obtained in Example 1 and the ZnFe2O4 catalyst obtained in Comparative Example 1 were used as representatives for further performance evaluation and mechanism analysis.

[0146] Figure 4 The PDS system represents the removal of TC by PDS oxidant alone; the ZnFe2O4 and CuO / ZnFe2O4 systems represent the removal of TC by ZnFe2O4 and CuO / ZnFe2O4 catalysts alone; and the ZnFe2O4 / PDS and CuO / ZnFe2O4 / PDS systems represent the removal of TC by PDS activated by ZnFe2O4 and CuO / ZnFe2O4 catalysts, respectively. Figure 4As shown, when PDS, ZnFe2O4, and CuO / ZnFe2O4 were added individually, the TC degradation rates within 60 minutes were only 29.64%, 46.50%, and 44.74%, respectively. This indicates that the inherent oxidation capacity of PDS and the adsorption capacity of ZnFe2O4 and CuO / ZnFe2O4 are insufficient to achieve efficient TC degradation. When ZnFe2O4 and PDS were used simultaneously, the TC removal efficiency of the ZnFe2O4 system did not significantly improve. However, the TC removal efficiency in the ZnFe2O4 / PDS system was significantly better than that in the PDS system and the CuO / ZnFe2O4 system, revealing the driving force of CuO / ZnFe2O4 on the activation of PDS and proving that the CuO / ZnFe2O4 catalyst has high catalytic performance.

[0147] Figure 5 The TC degradation rate curves of the CuO / ZnFe2O4 / PDS system at different initial pH values ​​show that the TC degradation efficiency is basically unaffected by changes in the initial pH value within the pH range of 3.0 to 9.0. This indicates that the CuO / ZnFe2O4 catalyst has a wide pH operating window (pH 3.0 to pH 9.0).

[0148] Ethanol (EtOH) was selected as the reactive oxygen species for hydroxyl radicals (·OH) and sulfate radicals (SO4). ·- Furfuryl alcohol (FFA) acts as a quencher for ·OH and singlet oxygen (OH). 1 O2) quenchers were added to ZnFe2O4 / PDS and CuO / ZnFe2O4 / PDS reaction systems, respectively. The inhibition rates of the quenchers were as follows: Figure 6 As shown. Compared with the blank control group without quencher, EtOH and FFA both inhibited the degradation efficiency of TC to some extent in both reaction systems. The quenching experiment results show that the loading of CuO significantly increased the proportion of FFA inhibition, indicating that CuO introduced quenching agent. 1 The O2 non-radical oxidation pathway is utilized. Therefore, compared with ZnFe2O4 / PDS, the CuO / ZnFe2O4 / PDS system exhibits better reaction selectivity.

[0149] (4) Salt tolerance test of the oxidation system

[0150] The test results of Example 3 were analyzed. Figure 7The bar chart shows the TC removal rate of the CuO / ZnFe2O4 / PDS system after 60 minutes of reaction under the condition of coexistence of different inorganic salt ions (each with a concentration of 500mM). As can be seen from the figure, the TC removal rate is stable at around 80%, which indicates that the degradation performance of the CuO / ZnFe2O4 / PDS system is basically unaffected by the coexisting inorganic salt ions, and it has high salt tolerance, making it suitable for various high-salt organic wastewaters.

[0151] (5) Chlorine resistance test of oxidation system

[0152] The test results for sodium chloride as the sodium salt in Example 3 were analyzed. Figure 8 For the CuO / ZnFe2O4 / PDS system with different concentrations of Cl - Under coexistence conditions, a bar chart of TC removal rates after 60 minutes of reaction showed that the TC removal rate remained stable between 78% and 88%, and even increased in Cl. - Even in extremely high salinity environments with concentrations as high as 1000 mM, the TC removal rate remains as high as 83%.

[0153] Therefore, the CuO / ZnFe2O4 catalyst has excellent salt and chlorine resistance, and is fully capable of achieving efficient and low-consumption treatment of high-salt organic wastewater.

[0154] (6) Stability performance test

[0155] The test results of Example 4 were analyzed, such as... Figure 9 As shown, after 5 cycles, the TC removal rate of the CuO / ZnFe2O4 catalyst remained stable at over 75%, indicating that the CuO / ZnFe2O4 catalyst has good stability.

[0156] In summary, the CuO / ZnFe2O4 catalyst provided by this invention possesses superior salt tolerance, excellent catalytic activity, and stability, and can effectively react with Cl... - It maintains a TC removal rate of over 80% in water environments with concentrations as high as 1000 mM, and the removal rate remains stable at over 75% after 5 cycles. Therefore, this material can be used as a catalyst to activate various oxidants such as persulfate, achieving efficient and low-consumption treatment of high-salt organic wastewater.

[0157] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for treating high-salt, recalcitrant organic wastewater, characterized in that, Includes the following steps: An oxidant and a CuO / ZnFe2O4 catalyst were added to a high-salinity water body containing organic pollutants to carry out a reaction; The catalyst is CuO nanoparticles supported on the surface of a sheet-like spinel metal oxide ZnFe2O4. The preparation method of the catalyst is as follows: A) A mixed metal salt solution containing zinc, iron, and copper salts is heated and stirred in a water bath. During this process, a chelating agent is added and the temperature is increased to carry out a sol-gel reaction to obtain the precursor. B) The precursor is dried and calcined to obtain a CuO / ZnFe2O4 catalyst; The organic pollutants include tetracycline, acetaminophen, bisphenol A, and 4-chlorophenol, with concentrations ranging from 5.0 to 20.0 mg / L. The salt ions in the high-salt water body include one or more of chloride ions, dihydrogen phosphate ions, bicarbonate ions, and nitrate ions, with a concentration of 100 mM to 1000 mM.

2. The processing method according to claim 1, characterized in that, The zinc salt is one of zinc acetate, zinc nitrate, zinc sulfate, and zinc chloride; The iron salt is one of ferric acetate, ferric nitrate, ferric sulfate, and ferric chloride; The copper salt is one of copper acetate, copper nitrate, copper sulfate, and copper chloride; The molar ratio of the zinc salt, iron salt, and copper salt is (0.5~2.0):(0.5~2.0):(0.5~2.0).

3. The processing method according to claim 1, characterized in that, The chelating agent is selected from at least one of citric acid, glycine, oxalic acid, ethylenediaminetetraacetic acid, and polyvinylpyrrolidone; The molar amount of the chelating agent used is the sum of the amounts of zinc salt, iron salt, and copper salt. The water bath heating temperature is 60℃~90℃, and the time is 5h~6h; The chelating agent is added after heating in a 60°C water bath and stirring for 1 hour. The heating process takes place 2 hours after adding the chelating agent and stirring thoroughly.

4. The processing method according to claim 1, characterized in that, The drying temperature is 60~90℃, and the time is 18h~24h; The calcination conditions are as follows: the precursor is heated from room temperature to 400℃~500℃ at a rate of 3~6℃ / min and held for 2~4 hours, followed by natural cooling.

5. The processing method according to claim 1, characterized in that, The catalyst is added at a rate of 0.05 g / L to 0.20 g / L. The oxidant is one of persulfate, permonsulfate, hydrogen peroxide, or periodate, and the dosage is 0.2 mM to 2.0 mM.

Citation Information

Patent Citations

  • Application of spinel ferrite catalyst and method for urging persulfate to generate free radicals to catalytically degrade organic matters

    CN103030208A

  • Nanocrystalline copper oxide / ferrite composite porous fiber electrode material and preparation method and application thereof

    CN103762087A